Nonionic silicone modified acrylate emulsion and preparation method thereof

Through the formulation and process of non-ionic silicone modified acrylate emulsion, the problem of poor emulsion bonding performance caused by anionic emulsifiers is solved, high adhesion and environmentally friendly production are achieved, and it is suitable for glass substrates.

CN116675805BActive Publication Date: 2024-11-26SHANDONG TELONGPU NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310838878.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-10
Publication Date
2024-11-26
Estimated Expiration
2043-07-10

AI Technical Summary

Technical Problem

In the prior art, anionic emulsifier initiates hydrolysis and polycondensation of silane coupling agent or vinyl coupling agent during emulsion polymerization, resulting in poor adhesion performance between the emulsion and the glass substrate.

Method used

Using the non-ionic silicone modified acrylate emulsion formula, the polycondensation of double bond silane or epoxy silane is avoided by mixing specific proportions and process steps of monomers, silane coupling agents, initiators, organic solvents and emulsifiers. Using organic peroxides or azo initiators, combined with high-speed stirring and shearing technology, a high-adhesion emulsion was prepared.

Benefits of technology

Improve the adhesion performance between the emulsion and the glass substrate, improve the utilization rate of silane coupling agent, reduce the amount of emulsifier, simplify the preparation steps, and realize a green and environmentally friendly production process, and the dispersion and stability of the emulsion good.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004329874540000061
    Figure BDA0004329874540000061
Patent Text Reader

Abstract

The present invention belongs to the technical field of resin or emulsion preparation, and specifically relates to a non-ionic silicone modified acrylic emulsion and a preparation method thereof. The emulsion is made of the following effective raw materials in parts by weight: 100 to 120 parts of mixed monomers, 1 to 2 parts of silane coupling agents, 0.3 to 1.2 parts of initiators, 35 to 50 parts of organic solvents, 1 to 2 parts of N,N-dimethylethanolamine, and 5 to 12 parts of emulsifiers. The non-ionic silicone modified emulsion avoids the catalytic hydrolysis and polycondensation of the coupling agent, effectively increases the effective silanol content in the emulsion, and has better adhesion to the substrate. The emulsion system is green and environmentally friendly as a whole, and has no VOC or HAPs emissions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of resin or emulsion preparation, and specifically relates to a nonionic silicone-modified acrylate emulsion and a preparation method thereof. Background Art

[0002] In order to improve the adhesion to substrates such as glass, silane coupling agents are usually directly added or vinyl coupling agents are added to participate in the polymerization during the emulsion polymerization process. At present, the emulsion polymerization method of the silicone-modified acrylic emulsion emulsifier, such as a styrene-acrylic emulsion and a preparation method thereof for simultaneously modifying two silane coupling agents disclosed in CN2010102928469, usually adopts anionic and non-ionic emulsifiers, and commonly used anionic emulsifiers such as sodium dodecylbenzene sulfonate and sodium dodecyl sulfate, and the initiator is persulfate, which will generate hydrogen ions when heated in water. However, the anionic emulsifier and hydrogen ions will promote the hydrolysis and polycondensation of the silane coupling agent or the vinyl coupling agent during the emulsion polymerization process, causing local cross-linking of the emulsion, and the cross-linked coupling agent will be filtered out in the subsequent processing steps, so the bonding performance with the glass substrate is poor. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a nonionic silicone modified acrylate emulsion, which has high bonding performance with a glass substrate. The present invention also provides a preparation method thereof, which is scientific, reasonable, simple and easy to implement.

[0004] The nonionic silicone-modified acrylic emulsion of the present invention is made of the following effective raw materials in parts by weight:

[0005] 100-120 parts of mixed monomer, 1-2 parts of silane coupling agent, 0.3-1.2 parts of initiator, 35-50 parts of organic solvent, 1-2 parts of N,N-dimethylethanolamine, 5-12 parts of emulsifier;

[0006] The mixed monomer is composed of at least two of butyl acrylate, methyl methacrylate, 2-hydroxyethyl acrylate, acrylic acid, methacrylic acid and hydroxyethyl methacrylate in any proportion;

[0007] The emulsifier is at least one of OP-10, OXO-1330, Tween 80, Peregal O-25, and Peregal O-30;

[0008] The initiator is an organic peroxide initiator or an azo initiator;

[0009] Silane coupling agent monomers contain double bond silane or epoxy silane.

[0010] The invention improves the formula of the emulsion, avoids the condensation polymerization catalysis of double-bond silane or epoxy silane, thereby ensuring the effective silanol content in the emulsion, so that the emulsion has higher adhesion to the glass substrate.

[0011] Preferably, every 100 parts by weight of the mixed monomers include 1 to 5 parts of acrylic acid, 45 to 55 parts of butyl acrylate and 40 to 50 parts of methyl methacrylate, calculated in parts by weight.

[0012] The silane coupling agent monomer is preferably at least one of vinyl triethoxysilane, 3-(methacryloxy)propyl triethoxysilane, 3-(methacryloxy)propyl methyl diethoxy silane, 3-glycidyloxypropyl methyl diethoxy silane and allyl glycidyl trimethoxy silane.

[0013] Preferably, the initiator is azobisisobutyronitrile, benzoyl peroxide, etc.

[0014] Preferably, the organic solvent is at least one of ethylene glycol diethyl ether, ethylene glycol butyl ether, propylene glycol butyl ether and acrylic acid.

[0015] Preferably, the emulsifier is at least one of OP-10, OXO-1330, Tween 80, Peregal O-25, and Peregal O-30.

[0016] Preferably, the emulsifiers are OP-10 and OXO-1330, and the mass ratio of OP-10 to OXO-1330 is 1:2.

[0017] Preferably, the amount of N,N-dimethylethanolamine used is 60% to 80% of the amount of the carboxylic acid.

[0018] The method for preparing the nonionic silicone-modified acrylate emulsion of the present invention comprises the following steps:

[0019] (1) adding 15% to 20% of the total amount of the mixed monomer and 15% to 20% of the total amount of the silane coupling agent to an organic solvent, heating to 72 to 78° C. in an inert gas, adding 15% to 20% of the total amount of the initiator, and reacting for 10 to 30 minutes to obtain a seed prepolymer;

[0020] (2) the remaining mixed monomers, silane coupling agent and initiator are mixed evenly, the mixture is heated to 85-105° C., and the mixture is added to the seed prepolymer prepared in step (1), and the mixture is reacted for 2-3 hours to obtain a prepolymer resin;

[0021] (3) Add N,N-dimethylethanolamine to the prepolymer resin and stir; add an emulsifier and stir and shear; add water while stirring, and continue stirring after adding, to obtain a non-ionic silicone-modified acrylate emulsion.

[0022] Preferably, the stirring speed in step (3) is 1500 to 2000 r / min.

[0023] Preferably, in step (2), a constant pressure dropping funnel is used to drop liquid into the seed prepolymer obtained in step (1) at a uniform speed.

[0024] Preferably, the amount of water used in step (3) is 112% to 143% of the mass of the prepolymer resin.

[0025] The preparation method of the present invention effectively avoids the cross-linking of the coupling agent during the polymerization process and the emulsification process. The organic solvent during the polymerization can itself serve as an emulsifier and does not need to be removed after the reaction is completed, thereby reducing the amount of the emulsifier and simplifying the preparation steps. The content of effective silanol groups in the modified emulsion is guaranteed. The emulsification process can avoid agglomeration and make the emulsion more uniform through stirring and shearing, thereby improving the stability of the entire system.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The emulsion of the present invention has good adhesion to glass substrates.

[0028] (2) The present invention has a high utilization rate of the silane coupling agent and a high effective content when the added amount is small.

[0029] (3) The present invention uses an environmentally friendly organic solvent for polymerization. The organic solvent itself can act as an emulsifier. After the reaction is completed, there is no need to remove the organic solvent, which reduces the amount of emulsifier used and simplifies the preparation steps.

[0030] (4) The emulsification process of the present invention is carried out under high-speed stirring and shearing, and the obtained emulsion has good dispersibility and good stability.

[0031] (5) The nonionic silicone modified emulsion prepared by the present invention is green and environmentally friendly, and has no VOC and HAPs emissions. DETAILED DESCRIPTION

[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with embodiments.

[0033] It should be noted that all raw materials used in the examples are commercially available unless otherwise specified.

[0034] Example 1

[0035] The preparation method of the nonionic silicone-modified acrylate emulsion of the present invention comprises the following steps:

[0036] The weighed mixed monomers, silane coupling agent and initiator are divided into two parts and added in two steps.

[0037] (1) 12.4 g of butyl acrylate, 11 g of methyl methacrylate, 0.6 g of acrylic acid and 0.4 g of 3-(methacryloyloxy)propyltriethoxysilane were added to 40 g of propylene glycol butyl ether, and nitrogen was introduced to replace the air; the temperature was raised to 75±3° C., 0.122 g of azobisisobutyronitrile was added, and the reaction was carried out for 30 minutes to obtain a seed prepolymer;

[0038] In this step, the amount of the mixed monomer (butyl acrylate, methyl methacrylate and acrylic acid), the silane coupling agent (3-(methacryloyloxy)propyltriethoxysilane) and the initiator (azobisisobutyronitrile) is 20% of the total amount.

[0039] (2) The remaining 49.6 g of butyl acrylate, 44 g of methyl methacrylate, 2.4 g of acrylic acid, 1.6 g of 3-(methacryloyloxy)propyltriethoxysilane, and 0.488 g of azobisisobutyronitrile were mixed evenly, and the mixture was heated to 95±5° C. and uniformly dripped into the seed prepolymer prepared in step (1) using a constant pressure dropping funnel for 2 h. The mixture was kept warm for 1 h to obtain a prepolymer resin.

[0040] (3) 1.30 g of N, N-dimethylethanolamine was added to 100 g of prepolymer resin for neutralization, and the pH was adjusted to 8.0 ± 0.5. The rotation speed was 1500 r / min and the mixture was stirred for 30 min. An emulsifier was added, and the amount of the emulsifier was 2 g OP-10 and 4 g OXO-1330. The rotation speed was 2000 r / min and the mixture was stirred and sheared for 10 min. While stirring, 120 g of water was added dropwise using a constant pressure dropping funnel. The addition was completed within 2 h. After the addition was completed, stirring was continued for 30 min to obtain a non-ionic silicone-modified acrylate emulsion.

[0041] Example 2

[0042] The preparation method of the nonionic silicone-modified acrylate emulsion according to the present invention comprises the following steps:

[0043] The weighed mixed monomers, silane coupling agent and initiator are divided into two parts and added in two steps.

[0044] (1) 12.4 g of butyl acrylate, 11 g of methyl methacrylate, 0.6 g of acrylic acid and 0.4 g of 3-(methacryloyloxy)propyltriethoxysilane were added to 40 g of propylene glycol butyl ether, and nitrogen was introduced to replace the air; the temperature was raised to 75±3° C., 0.122 g of benzoyl peroxide was added, and the reaction was carried out for 30 minutes to obtain a seed prepolymer;

[0045] In this step, the amount of the mixed monomer, the silane coupling agent and the initiator is 20% of the total amount.

[0046] (2) The remaining 49.6 g of butyl acrylate, 44 g of methyl methacrylate, 2.4 g of acrylic acid, 1.6 g of vinyl triethoxysilane and 0.488 g of benzoyl peroxide were mixed evenly, and the mixture was heated to 95±5° C. and uniformly dripped into the seed prepolymer prepared in step (1) using a constant pressure dropping funnel for 2 h. The mixture was kept warm for 1 h to obtain a prepolymer resin.

[0047] (3) 1.22 g of N, N-dimethylethanolamine was added to 100 g of prepolymer resin for neutralization, and the pH was adjusted to 7.0 ± 0.5. The rotation speed was 1500 r / min and the mixture was stirred for 30 min. An emulsifier was added, and the amount of the emulsifier was 2 g of OP-10 and 4 g of OXO-1330. The rotation speed was 2000 r / min and the mixture was stirred and sheared for 10 min. While stirring, 120 g of water was added dropwise using a constant pressure dropping funnel, and the addition was completed within 2 h. After the addition was completed, stirring was continued for 30 min to obtain a non-ionic silicone-modified acrylate emulsion.

[0048] Example 3

[0049] The preparation method of the nonionic silicone-modified acrylate emulsion according to the present invention comprises the following steps:

[0050] The weighed mixed monomers, silane coupling agent and initiator are divided into two parts and added in two steps.

[0051] (1) 9.3 g of butyl acrylate, 8.25 g of methyl methacrylate, 0.45 g of acrylic acid and 0.3 g of 3-(methacryloyloxy)propyltriethoxysilane were added to 40 g of propylene glycol butyl ether, and nitrogen was introduced to replace the air; the temperature was raised to 75±3° C., 0.122 g of azobisisobutyronitrile was added, and the reaction was carried out for 30 minutes to obtain a seed prepolymer;

[0052] In this step, the amount of the mixed monomer and the silane coupling agent is 15% of the total amount, and the amount of the initiator is 20% of the total amount.

[0053] (2) The remaining 52.7 g of butyl acrylate, 46.75 g of methyl methacrylate, 2.55 g of acrylic acid, 1.7 g of allyl glycidyl ether trimethoxysilane and 0.488 g of azobisisobutyronitrile were mixed evenly and the mixture was heated to 100±5° C. The seed prepolymer prepared in step (1) was added dropwise at a uniform speed using a constant pressure dropping funnel for 2 h and kept warm for 1 h to obtain a prepolymer resin.

[0054] (3) 1.22 g of N,N-dimethylethanolamine was added to 100 g of prepolymer resin for neutralization, and the pH was adjusted to 8.0±0.5. The speed was 1500 r / min and the mixture was stirred for 30 min. An emulsifier was added, and the amount of the emulsifier was 2.5 g of OP-10 and 4.5 g of Tween 80. The speed was 2000 r / min and the mixture was stirred and sheared for 10 min. While stirring, 120 g of water was added dropwise using a constant pressure dropping funnel. The addition was completed within 2 h. After the addition was completed, stirring was continued for 30 min to obtain a non-ionic silicone-modified acrylate emulsion.

[0055] Example 4

[0056] The preparation method of the nonionic silicone-modified acrylate emulsion according to the present invention comprises the following steps:

[0057] The weighed mixed monomers, silane coupling agent and initiator are divided into two parts and added in two steps.

[0058] (1) 9.3 g of butyl acrylate, 8.25 g of methyl methacrylate, 0.45 g of acrylic acid and 0.3 g of 3-(methacryloyloxy)propyltriethoxysilane were added to 40 g of propylene glycol butyl ether, and nitrogen was introduced to replace the air; the temperature was raised to 75±3° C., 0.147 g of azobisisobutyronitrile was added, and the reaction was carried out for 30 minutes to obtain a seed prepolymer;

[0059] In this step, the amount of the mixed monomer, the silane coupling agent and the initiator is 15% of the total amount.

[0060] (2) The remaining 52.7 g of butyl acrylate, 46.75 g of methyl methacrylate, 2.55 g of acrylic acid, 1.7 g of 3-(methacryloyloxy)propyltriethoxysilane and 0.829 g of azobisisobutyronitrile were mixed evenly, and the mixture was heated to 90±5° C. and uniformly dripped into the seed prepolymer prepared in step (1) using a constant pressure dropping funnel for 2 h. The mixture was kept warm for 1 h to obtain a prepolymer resin.

[0061] (3) 1.22 g of N,N-dimethylethanolamine was added to 100 g of prepolymer resin for neutralization, and the pH was adjusted to 7.0±0.5. The speed was 1500 r / min and the mixture was stirred for 30 min. An emulsifier was added, and the amount of the emulsifier was 2.5 g of Perchlorate O-30 and 4.5 g of Tween 80. The mixture was stirred and sheared for 10 min at a speed of 2000 r / min. 115 g of water was added dropwise using a constant pressure dropping funnel while stirring. The mixture was added dropwise over a period of 2 h. After the addition was completed, stirring was continued for 30 min to obtain a non-ionic silicone-modified acrylate emulsion.

[0062] Example 5

[0063] The preparation method of the nonionic silicone-modified acrylate emulsion according to the present invention comprises the following steps:

[0064] The weighed mixed monomers, silane coupling agent and initiator are divided into two parts and added in two steps.

[0065] (1) 11.16 g of butyl acrylate, 9.9 g of methyl methacrylate, 0.54 g of acrylic acid and 0.3 g of 3-(methacryloyloxy)propyltriethoxysilane were added to 40 g of propylene glycol butyl ether, and nitrogen was introduced to replace the air; the temperature was raised to 75±3° C., 0.122 g of azobisisobutyronitrile was added, and the reaction was carried out for 30 minutes to obtain a seed prepolymer;

[0066] In this step, the amount of the mixed monomer is 18% of the total amount; the amount of the silane coupling agent is 15% of the total amount; and the amount of the initiator is 20% of the total amount.

[0067] (2) The remaining 50.84 g of butyl acrylate, 45.1 g of methyl methacrylate, 2.46 g of acrylic acid, 1.64 g of 3-(methacryloyloxy)propyltriethoxysilane and 0.488 g of azobisisobutyronitrile were mixed evenly and heated to 95±5° C. The seed prepolymer prepared in step (1) was added dropwise at a uniform speed using a constant pressure dropping funnel for 2 h and kept warm for 1 h to obtain a prepolymer resin.

[0068] (3) 1.30 g of N, N-dimethylethanolamine was added to 100 g of prepolymer resin for neutralization, and the pH was adjusted to 8.0 ± 0.5. The rotation speed was 1500 r / min and the mixture was stirred for 30 min. An emulsifier was added, and the emulsifier dosage was 2 g OP-10 and 4 g Perpenta O-25. The rotation speed was 2000 r / min and the mixture was stirred and sheared for 10 min. While stirring, 115 g of water was added dropwise using a constant pressure dropping funnel, and the addition was completed within 2 h. After the addition was completed, the mixture was stirred for 30 min to obtain a non-ionic silicone-modified acrylate emulsion.

[0069] Comparative Example 1

[0070] (1) 62 g of butyl acrylate, 55 g of methyl methacrylate, 0.6 g of acrylic acid, 1 g of 3-(methacryloyloxy)propyltriethoxysilane, 1 g of OP-10 and 2 g of OXO-1330 were added to 70 g of water and stirred at 9000 r / min for 10 min using a homogenizer to prepare a stable pre-milk.

[0071] (2) Weigh 0.65 g of ammonium persulfate and add 20 g of water to dissolve and disperse evenly to prepare an initiator aqueous solution.

[0072] (3) Add 1g OP-10 and 2g OXO-1330 emulsifiers and 0.72g NaHCO3 to 50g water and heat it to 75±5℃. Add 9g pre-emulsified emulsion and 3g initiator aqueous solution. When the flask turns blue, add the pre-emulsified emulsion and initiator aqueous solution dropwise while keeping the temperature in the flask at 78±3℃. The addition is completed in 2.5 hours.

[0073] (4) Add 1 g of 3-(methacryloyloxy)propyltriethoxysilane and 3 g of an initiator aqueous solution, keep warm for 1 hour, and then cool and filter.

[0074] Comparative Example 2

[0075] (1) 62 g of butyl acrylate, 55 g of methyl methacrylate, 0.6 g of acrylic acid, 1 g of vinyltrimethoxysilane, 1 g of OP-10 and 2 g of OXO-1330 were added to 70 g of water and stirred at 9000 r / min for 10 min using a homogenizer to prepare a stable pre-milk.

[0076] (2) Weigh 0.65 g of ammonium persulfate and add 20 g of water to dissolve and disperse evenly to prepare an initiator aqueous solution.

[0077] (3) Add 1g OP-10, 2g OXO-1330 and 0.72g NaHCO3 to 50g water and heat it to 75°C. Add 9g pre-emulsion and 3g initiator aqueous solution. When the flask turns blue, add the emulsion and initiator aqueous solution dropwise while keeping the temperature in the flask at 75-80°C. The addition is completed in 2.5 hours.

[0078] (4) Add 1 g of vinyltrimethoxysilane and 3 g of initiator aqueous solution, keep warm for 1 hour, then cool and filter.

[0079] Performance Testing

[0080] The bonding performance of Examples 1 to 5 and Comparative Examples 1 and 2 was tested in accordance with GB / T 13477.18-2002. The test results are shown in Tables 1 and 2:

[0081] Table 1: Preparation of non-ionic emulsion and substrate bonding experiment

[0082]

[0083] Table 2: Comparative test of bonding of the emulsion prepared in Example 1 and the emulsion prepared in the comparative example on glass

[0084] Example 1 0.90MPa Comparative Example 1 0.45MPa Comparative Example 2 0.42MPa

[0085] As can be seen from Table 1, the present invention has excellent adhesion to the substrate, especially on the glass substrate. As can be seen from Table 2, the adhesion of the non-ionic silicone modified emulsion prepared in Example 1 of the present invention on glass is significantly better than that in Comparative Examples 1 and 2, indicating that the anions and cations catalyzed the polycondensation of silanol in water during the preparation of Comparative Examples 1 and 2, making the silicone monomers in the long polymer chain more inclined to be closer. In the first stage of the emulsion prepared in this Example 1, the silicone monomers in the long polymer chain did not participate in the hydrolysis and polycondensation, making the distribution more uniform and the steric hindrance greater, and then the effective silicone hydroxyl groups can be effectively retained in the second step of emulsification, that is, the effective silicon content of the emulsion is higher and the bonding strength is significantly improved.

Claims

1. Nonionic silicone modified acrylate emulsion, characterized in that: It is prepared from the following effective raw materials in parts by weight: 100-120 parts of mixed monomers, 1-2 parts of silane coupling agents, 0.3-1.2 parts of initiators, 35-50 parts of organic solvents, 1-2 parts of N,N-dimethylethanolamine, and 5-12 parts of emulsifiers; The mixed monomer is composed of at least two of butyl acrylate, methyl methacrylate, 2-hydroxyethyl acrylate, acrylic acid, methacrylic acid and hydroxyethyl methacrylate in any proportion; The emulsifier is at least one of OP-10, OXO-1330, Tween 80, Peregal O-25, and Peregal O-30; The initiator is an organic peroxide initiator or an azo initiator; Silane coupling agent monomers contain double bond silane or epoxy silane; The emulsifiers are OP-10 and OXO-1330, and the mass ratio of OP-10 to OXO-1330 is 1:2; Use N, N-methylethanolamine to neutralize to pH 6.5-8.5; The preparation method of the nonionic silicone-modified acrylate emulsion comprises the following steps: (1) 15% to 20% of the total amount of the mixed monomer and 15% to 20% of the total amount of the silane coupling agent are added to an organic solvent, the temperature is raised to 72 to 78° C. in an inert gas, 15% to 20% of the total amount of the initiator is added, and the reaction is carried out for 10 to 30 minutes to obtain a seed prepolymer; (2) the remaining mixed monomers, silane coupling agent and initiator are mixed evenly, the mixture is heated to 85-105° C., and the mixture is added to the seed prepolymer prepared in step (1), and the mixture is reacted for 2-3 hours to obtain a prepolymer resin; (3) Add N,N-dimethylethanolamine to the prepolymer resin and stir; add an emulsifier and stir and shear; add water while stirring, and continue stirring after adding, to obtain a non-ionic silicone modified acrylate emulsion; The stirring speed of step (3) is 1500-2000 r / min; The silane coupling agent monomer contains at least one of 3-(methacryloyloxy)propyltriethoxysilane, 3-(methacryloyloxy)propylmethyldiethoxysilane, 3-glycidyloxypropylmethyldiethoxysilane and allyl glycidyl ether trimethoxysilane; In step (2), a constant pressure dropping funnel is used to drop the seed prepolymer obtained in step (1) at a uniform speed; The amount of water used in step (3) is 112% to 143% of the mass of the prepolymer resin.

2. The nonionic silicone-modified acrylate emulsion according to claim 1, characterized in that: Every 100 parts by weight of the mixed monomers includes 1 to 5 parts of acrylic acid, 45 to 55 parts of butyl acrylate and 40 to 50 parts of methyl methacrylate, calculated in parts by weight.

3. The nonionic silicone-modified acrylate emulsion according to claim 1, characterized in that: The initiator is azobisisobutyronitrile or benzoyl peroxide.