A method for preparing a soft-pack battery cell and a soft-pack battery cell thereof

By using weakly acidic liquid rinsing and isolating film stacking and hot-pressing encapsulation in the preparation of lithium-ion battery cells, the problem of difficult removal of non-magnetic metal impurities in the cells is solved, and the actual reduction of impurity content in the cells is achieved. and cycle performance improvements.

CN116706255BActive Publication Date: 2024-10-25JIANGSU TIANHE ENERGY STORAGE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310817937.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-05
Publication Date
2024-10-25
Estimated Expiration
2043-07-05

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively reduce the content of non-magnetic metal impurities in lithium-ion battery cells, resulting in increased internal resistance and shortened cell cycle life, and the cost of removing impurities is high.

Method used

A weakly acidic liquid rinsing method is used to remove soluble metal impurities during the cell preparation process. By laminating with the isolation film and hot-pressing the package, combined with the baking and electrolyte infiltration steps, all soluble metal impurities inside the cell can be removed in one step. Impurities.

Benefits of technology

It reduces the metal impurity content of the battery core and improves the cycle performance and life of the battery core. It is easy to operate and does not require large-scale water washing or impurity removal devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116706255B_ABST
    Figure CN116706255B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of battery cell preparation, and relates to a method for preparing a soft-package battery cell and a soft-package battery cell thereof. The method for preparing a soft-package battery cell comprises the following steps: S1: preparing a positive electrode sheet and a negative electrode sheet; S2: stacking the positive electrode sheet and the negative electrode sheet and a separator in order, hot pressing the bare battery cell, using an aluminum-plastic film to seal the top and side, and placing the battery cell in an environment of 85±5°C for baking for 12±0.5h; S3: injecting a rinse solution, sealing, standing for 2‑24h, pouring out the rinse solution, and then replacing; etc. The present invention adopts an impurity removal method in the battery cell preparation stage, and removes soluble metal impurities in the entire battery cell by rinsing with a weak acidic liquid. The operation difficulty is low, and no large-scale water washing or impurity removal device is required. The soluble impurities of all materials can be removed in one step, and the metal impurity content in the battery cell is truly reduced, thereby improving the battery cell cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery cell preparation, and relates to a method for preparing a soft-pack battery cell and the soft-pack battery cell. Background Art

[0002] In recent years, lithium-ion batteries have been widely used in electronic products, electric vehicles, energy storage power supplies and other fields due to their advantages such as high energy density, long cycle life and green environmental protection. Among them, the high energy density and long cycle life of lithium-ion batteries are inseparable from the metal impurity content of the system. In order to give full play to the high capacity and long cycle life of the battery, the metal impurity content of the system material must be reduced. At present, the reduction of impurity content in the battery is mainly controlled at the material preparation level, such as controlling the impurity content of the precursor of the synthetic material, demagnetization in the material synthesis stage, etc. The above materials are only controlled at certain stages of the synthesis, and the magnetic impurities in the material are mostly controlled. It is difficult to eliminate some non-magnetic metal compound impurities. These impurities dissolve and adsorb on the negative electrode side surface during the cycle, destroying and catalyzing the formation of SEI, thereby increasing the internal resistance and consuming lithium ions, shortening the cycle life of the battery. In addition, there are many types of raw materials for the battery, and each material is impurity-removed, which is costly. Therefore, it is urgent to design a soft-pack battery preparation process that can overcome the above defects to reduce impurities and improve the cycle.

[0003] In order to overcome the shortcomings of the prior art, people have proposed various solutions through continuous exploration. For example, a Chinese patent discloses a method for preparing a battery cell [application number: 201410398185.6], which includes the following steps: cutting a linear array of first notches at the edge and / or inside of the first current collector along the longitudinal direction of the first current collector, applying a first slurry containing a first active material and drying it, and cold pressing it to prepare a first pole piece; cutting a linear array of second notches corresponding to and matching the notches of the first current collector at a position corresponding to the first current collector of the second current collector along the longitudinal direction of the second current collector, applying a second slurry containing a second active material and drying it, and cold pressing it to prepare a second pole piece; setting a first pole ear; setting a second pole ear; setting an isolation film to form a stack; winding the stack into a battery cell, the first notch of the corresponding first pole piece and the second notch of the corresponding second pole piece form a cut-out portion, and the corresponding edges of the first notch of the corresponding first pole piece and the second notch of the corresponding second pole piece are aligned. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a soft-pack battery cell and a soft-pack battery cell thereof in view of the above problems.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for preparing a soft-pack battery cell, characterized in that it comprises the following steps:

[0007] S1: Preparation of positive electrode sheet and negative electrode sheet;

[0008] S2: stack the positive electrode sheet, the negative electrode sheet and the isolation film in order, hot-press the bare cell, seal the top and side with aluminum-plastic film, and bake the cell at 85±5°C for 12±0.5h;

[0009] S3: inject the rinse solution, seal the bottle, let it stand for 2-24 hours, pour out the rinse solution, and then replace it;

[0010] S4: injecting electrolyte, vacuum sealing, and infiltration at 45-85℃ for 8-48h before forming; step S5: after heating and aging for 5.5-6.5h, vacuuming, secondary sealing, volume separation and testing, extracting excess electrolyte from the battery cell produced in step S4, trimming and conducting insulation testing and volume separation.

[0011] In the above-mentioned method for preparing a soft-pack battery cell, in the step S3, the rinsing solution may be an organic solution or a weak acid solution, and the rinsing time may be 2-48 hours.

[0012] In the above-mentioned method for preparing a soft-pack battery cell, in the step S3, the electrolyte is injected, the opening is sealed, and the mixture is left to stand for 18-24 hours, the rinse solution is poured out, and the mixture is rinsed with the electrolyte for 2-4 more times.

[0013] In the above-mentioned method for preparing a soft-pack battery cell, step S4: injecting electrolyte to reach the target mass, vacuum sealing, and forming after infiltration at 45-70°C for 18-24 hours; step S5: aging at 55°C-65°C for 5-7 hours, vacuuming, secondary sealing, volume separation and testing, extracting excess electrolyte from the battery cell produced in step S4, trimming it, performing insulation testing, and volume separation.

[0014] In the above-mentioned method for preparing a soft-pack battery cell, in the step S3, 0.006-0.01 mol / L HCl is injected, the opening is sealed, and the mixture is allowed to stand for 18-24 hours. The rinse solution is poured out, and the mixture is rinsed with DMC for 2-4 times and dried.

[0015] In the above-mentioned method for preparing a soft-pack battery cell, step S4: injecting electrolyte to reach the target mass, vacuum sealing, and forming after soaking at 45-65° C. for 18-24 hours.

[0016] In the above-mentioned method for preparing a soft-pack battery cell, step S5: after aging at 58°C-62°C for 5.5-6.5h, vacuumizing, secondary sealing, volume separation and testing, extracting excess electrolyte from the battery cell produced in S4, trimming and conducting insulation testing and volume separation.

[0017] In the above-mentioned method for preparing a soft-pack battery cell, after the battery cell is baked in step S2, S3 is skipped and the rinsing operation is cancelled.

[0018] In the above-mentioned method for preparing a soft-pack battery cell, after the battery cell is baked in step S2, step S4 is performed: injecting electrolyte, vacuum sealing, and soaking at 50-65° C. for 8-48 hours before forming.

[0019] In the above-mentioned method for preparing a soft-pack battery cell, step S5: after aging at 60° C. for 6 hours, vacuumizing, secondary sealing, volume separation and testing, extracting excess electrolyte from the battery cell produced in step S4, trimming and conducting insulation testing and volume separation.

[0020] Another aspect of the present invention also provides a soft-pack battery cell, which is prepared by the above method.

[0021] Compared with the prior art, the advantages of the present invention are:

[0022] 1. The present invention adopts an impurity removal method in the battery cell preparation stage, and removes soluble metal impurities in the entire battery cell by rinsing with a weak acidic liquid. The operation is easy and does not require large-scale water washing or impurity removal equipment.

[0023] 2. The present invention can remove soluble impurities of all materials in one step, truly reduce the content of metal impurities in the battery cell, and improve the cycle performance of the battery cell.

[0024] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the cycle data of Example 1.

[0026] Figure 2 It is a schematic diagram of the cycle data of Example 2.

[0027] Figure 3 It is a schematic diagram of the cycle data of Example 3.

[0028] Figure 4 It is a schematic diagram of the cycle data of Comparative Example 1. DETAILED DESCRIPTION

[0029] The present invention will be further described below in conjunction with the accompanying drawings.

[0030] like Figure 1-4 As shown, a method for preparing a soft-pack battery cell of the present invention comprises the following steps:

[0031] S1: Preparation of positive electrode sheet and negative electrode sheet;

[0032] S2: stack the positive electrode sheet, the negative electrode sheet and the isolation film in order, hot-press the bare cell, seal the top and side with aluminum-plastic film, and bake the cell at 85±5°C for 12±0.5h;

[0033] S3: inject the rinse solution, seal the bottle, let it stand for 2-24 hours, pour out the rinse solution, and then replace it;

[0034] S4: injecting electrolyte, vacuum sealing, and infiltration at 45-85℃ for 8-48h before forming; step S5: after heating and aging for 5.5-6.5h, vacuuming, secondary sealing, volume separation and testing, extracting excess electrolyte from the battery cell produced in step S4, trimming and conducting insulation testing and volume separation.

[0035] In the present invention, an impurity removal method is adopted in the battery cell preparation stage, and the soluble metal impurities inside the entire battery cell are removed by rinsing with a weak acidic liquid. The operation is easy and does not require a large-scale water washing or impurity removal device. The soluble impurities of all materials can be removed in one step, and the metal impurity content inside the battery cell is truly reduced, thereby improving the battery cell cycle performance.

[0036] Example 1

[0037] Combination Figure 1 As shown, the method for preparing the soft-pack battery cell of this embodiment includes the following steps:

[0038] S1: preparing positive electrode sheets and negative electrode sheets, the sizes of which are determined according to different battery models;

[0039] S2: stack the positive electrode sheet, the negative electrode sheet and the isolation film in order, hot-press the bare cell, seal the top and side with aluminum-plastic film, and bake the cell at 85±5°C for 12±0.5h;

[0040] S3: inject electrolyte, seal, let stand for 20 hours, pour out the rinse solution, and rinse with electrolyte three more times;

[0041] S4: Inject electrolyte to reach the target mass, evacuate and seal, and soak at 50-65℃ for 24h before forming;

[0042] S5: After heating to 55-60° C. and aging for 5.8 hours, vacuumizing, resealing, volume separation and testing are performed, and the excess electrolyte of the battery cell produced in step S4 is extracted, and the edges are trimmed, and the insulation test and volume separation are performed.

[0043] Example 2

[0044] Combination Figure 2 As shown, the method for preparing the soft-pack battery cell of this embodiment is different from that of Embodiment 1 in that:

[0045] Take Example 1 and bake the battery cell after step S2;

[0046] S3: Inject DMC, seal, let stand for 24 hours, pour out the rinse solution, rinse three more times with DMC, and dry.

[0047] S4: Inject electrolyte to reach the target mass, evacuate and seal, and soak at 55-65℃ for 24h before forming.

[0048] S5: After aging at 60°C for 6.5 hours, vacuumize, reseal, separate and test. Extract the excess electrolyte of the battery produced in step S4, trim and perform insulation test and separate.

[0049] Example 3

[0050] Combination Figure 3 As shown, the method for preparing the soft-pack battery cell of this embodiment is different from that of Embodiment 1 in that:

[0051] Take Example 1 and bake the battery cell after step S2;

[0052] S3: Inject 0.008 mol / L HCl, seal, let stand for 24 h, pour out the rinse solution, rinse three times with DMC, and dry.

[0053] S4: Inject electrolyte to reach the target mass, evacuate and seal, and soak at 45-65℃ for 24h before forming.

[0054] S5: After aging at 60°C for 6 hours, vacuumize, reseal, separate and test. Extract the excess electrolyte of the battery produced in step S4, trim and perform insulation test and separate.

[0055] Comparative Example 1

[0056] Combination Figure 4 As shown, after the battery cell is baked in Example 1, no rinsing operation is performed, and step S3 is skipped;

[0057] Step S4: inject electrolyte, evacuate and seal, and soak at 45-65°C for 8-48h before forming.

[0058] Step S5: After aging at 60°C for 6 hours, vacuumize, reseal, separate and test. Extract the excess electrolyte of the battery produced in step 04, trim and test the insulation, and separate.

[0059]

[0060] Compared with Example 1 and Comparative Example 1, the iron impurities on the negative electrode side of the battery cell after rinsing are significantly reduced after capacity division, and the capacity is higher, indicating that the amount of lithium consumed by the first SEI is reduced. Example 1 is cycled 4500 times, and the capacity retention rate is 90%. Comparative Example 1 is cycled 4000 times, and the capacity retention rate is 80%. The iron content on the negative electrode side is reduced, and the damage to SEI and re-catalytic generation are reduced, thereby improving the cycle performance.

[0061] By comparing Examples 1, 2, and 3, it is found that Example 1 has the best effect. After capacity division, the iron content on the negative electrode side is lower, the capacity is maximized, and the cycle effect is the best. The reason is that Example 1 increases the wetting effect, the electrolyte is more fully immersed, and the polarization is reduced.

[0062] In this way, impurity removal is achieved during the preparation stage of the battery cell. The soluble metal impurities inside the entire battery cell are removed by rinsing with a weak acidic liquid. The operation is easy and does not require large-scale water washing or impurity removal equipment. The soluble impurities of all materials can be removed in one step, and the metal impurity content inside the battery cell can be truly reduced to improve the cycle performance of the battery cell.

[0063] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways without departing from the spirit of the present invention.

Claims

1. A method for preparing a soft-pack battery cell, characterized in that: The steps include: S1: Preparation of positive electrode sheet and negative electrode sheet; S2: stack the positive electrode sheet, the negative electrode sheet and the isolation film in order, hot-press the bare cell, seal the top and side with aluminum-plastic film, and bake the cell at 85±5°C for 12±0.5h; S3: inject a rinse solution of 0.006-0.01 mol / L HCl, seal the tube, let stand for 18-24 hours, pour out the rinse solution, rinse again with dimethyl carbonate DMC for 2-4 times, and dry; S4: inject electrolyte, evacuate and seal, soak at 45-85℃ for 8-48h and then form; S5: After heating and aging for 5.5-6.5 hours, vacuumize, re-seal, divide the capacity and test, extract the excess electrolyte of the battery cell produced in the step S4, trim it, conduct insulation test and divide the capacity.

2. A method for preparing a soft-pack battery cell according to claim 1, characterized in that: Step S4: injecting electrolyte to reach the target quality, vacuum sealing, and forming after infiltration at 45-70℃ for 18-24h; Step S5: after aging at 55℃-65℃ for 5.5-6.5h, vacuuming, secondary sealing, volume separation and testing, extracting the excess electrolyte of the battery cell produced in step S4, trimming and conducting insulation testing and volume separation.

3. A method for preparing a soft-pack battery cell according to claim 1, characterized in that: Step S4: inject electrolyte to reach the target mass, evacuate and seal, and infiltrate at 45-65°C for 18-24h before forming.

4. A method for preparing a soft-pack battery cell according to claim 3, characterized in that: Step S5: After aging at 58°C-62°C for 5.5-6.5h, vacuumize, re-seal, separate and test, extract excess electrolyte from the battery cell produced in S4, perform edge trimming, insulation test and separate.

5. A soft-pack battery cell, characterized in that: It is prepared by the method according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Preparation method of electric core

    CN104157912A

  • Lithium ion battery electrolyte and battery production method

    CN104993175A

  • Lithium-ion battery baking and liquid-injection system and method

    CN106207271A

  • Lithium ion battery assembly method and lithium ion battery

    CN110690506A

  • Optimized preparation method of prefabricated SEI film on negative electrode surface of zinc ion lithium battery