Control methods for tin plating equipment
By sampling the tin-plated sheet along its width and conducting inductively coupled plasma testing, the tin-plating equipment was adjusted, which solved the problem of poor tin plating uniformity, improved the corrosion resistance and weldability of the tin-plated sheet, met customer needs, and reduced costs.
Patent Information
- Application Number
- CN202310685025.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-09
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-06-09
AI Technical Summary
Poor uniformity of tin plating on the surface of tinplate results in poor adhesion between the tin layer and the steel plate, as well as poor corrosion resistance and weldability, failing to meet the performance requirements of downstream customers.
By sampling the tin-plated plate along its width, the amount of tin plating is determined using inductively coupled plasma (ICP) testing. The tin plating equipment is then adjusted based on the comparison results, including adjusting the position of the tin plating anode, replacing the tin plating anode or the tin plating solution, and controlling the working condition of the tin plating equipment.
It improves the uniformity of tin plating on tinplate, enhances corrosion resistance and weldability, meets customer needs, and simplifies the experimental process and reduces costs.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of steel material preparation technology, specifically relating to a method for controlling tin plating equipment. Background Technology
[0002] Tinplate is made by plating a tin layer onto a thin steel plate. It has good corrosion resistance, stamping performance and welding performance, and has a bright and beautiful appearance, making it one of the commonly used materials for food packaging.
[0003] However, in actual production, the actual amount of tin plating on the surface of the tinplate usually differs from the preset amount, resulting in poor uniformity of tin plating on the steel plate surface. This leads to poor adhesion between the tin layer and the steel plate, poor corrosion resistance, poor weldability, and poor gloss, which fails to meet the performance requirements of downstream customers. Summary of the Invention
[0004] The purpose of this invention is to provide a method for controlling tin plating equipment to solve the problem of poor tin plating uniformity on tin-plated plates.
[0005] To achieve the above-mentioned objective, one embodiment of the present invention provides a method for controlling a tin plating equipment, including sequential sampling, measuring the tin plating amount of each sample, and controlling the tin plating equipment. In the sampling step, the tinplate is divided into a first region and a second region along a symmetry axis parallel to its length direction. Samples are cut from the first region and the second region according to the sampling method. Along the width direction of the tinplate, the length of each sample gradually increases from the side of the tinplate toward the midpoint along its width direction, and all samples have the same area. In the tin plating amount determination step, a beaker containing 60 mL of 30% hydrochloric acid solution is heated to 90°C. The sample is added to the beaker, and the heating temperature is maintained at 90°C until the surface of the tin-plated plate is completely dull or the solution in the beaker begins to turn yellow and produces a large number of bubbles. Heating is then stopped. The cooled solution is poured into a 100 mL volumetric flask, 5 drops of concentrated hydrochloric acid are added, and then deionized water is added to bring the volume to 100 mL. The tin ion concentration C in the volumetric flask is determined using inductively coupled plasma (ICP-CPS) measurement. i And convert it into the tin plating amount ρ of each sample. i ; In the tin plating equipment control step, the tin plating amount ρ of each sample is adjusted. i The tin plating amount ρ0 of the tin-plated plate is compared with the preset tin plating amount ρ0, and the tin plating equipment used in the tin plating process is adjusted according to the comparison result.
[0006] As a further improvement of one embodiment of the present invention, the sampling method includes: establishing an X-axis with one side of the tin-plated plate as the origin, and extending along the width direction of the tin-plated plate towards the other side; sequentially cutting samples from the origin along the X-axis towards the midpoint of the tin-plated plate along its width direction and numbering them in sequence, with the coordinates of the first and last ends of sample i along the X-axis being X... i 'and X i , where X i '=X i +ΔX i X1=0mm, ΔX i ≥ΔX i-1 1mm≤ΔX i ≤20mm; when i≤5, X i =X i-1 When i≥6, X i >X i-1 '.
[0007] As a further improvement to one embodiment of the present invention, when i=1~2, ΔX i =1mm; when i=3, ΔX i =2mm; when i=4~5, ΔX i =2~4mm.
[0008] As a further improvement to one embodiment of the present invention, the amount of tin plating ρ of each sample is... i The process of comparing the tin plating amount ρ0 with the preset tin plating amount of the tin-plated board and adjusting the tin plating equipment used in the tin plating process based on the comparison result specifically includes: When i≥6, the tin plating amount ρ of each sample i Compare with the preset tin plating amount ρ0; If i≥6, then ρ i If the fluctuation range exceeds the preset tin plating amount ρ0, then adjust the position of the tin plating anode or replace the tin plating anode.
[0009] As a further improvement to one embodiment of the present invention, if i ≥ 6, then ρ i If the fluctuation range exceeds the preset tin plating amount ρ0, check the dispersion performance of the tin plating solution and detect whether the impurities in the tin plating solution exceed the standard. If the dispersion performance of the tin plating solution is unqualified, and / or the impurities in the tin plating solution exceed the standard, the tin plating solution shall be replaced.
[0010] As a further improvement to one embodiment of the present invention, the amount of tin plating ρ of each sample is... i The process of comparing the tin plating amount ρ0 with the preset tin plating amount of the tin-plated plate and adjusting the tin plating equipment used in the tin plating process based on the comparison result specifically includes: If, among samples 1 to 5, the difference in tin plating amount between the sample and the board is Δρ i If the value is greater than 2ρ0, then adjust the position of the anode edge cover to increase the shielding area of the anode edge cover on the tin-plated anode. Among them, the difference in tin plating amount between the sample and the board is Δρ i =ρ i -ρ0.
[0011] As a further improvement to one embodiment of the present invention, the tin plating amount ρ of each sample... i Convert using the following formula: ρ i =50C i / S, where S is the area of the sample in mm. 2 C i The unit is mg / L; ρ i The unit is g / m 2 .
[0012] As a further improvement of one embodiment of the present invention, the area of the sample is S=200mm². 2 .
[0013] As a further improvement of one embodiment of the present invention, in the step of determining the amount of tin plating, the surface of the sample is wiped with alcohol before adding the sample to the beaker.
[0014] As a further improvement of one embodiment of the present invention, in the step of determining the amount of tin plating, when adding the sample to the beaker, the sample is cut into small pieces and added to the beaker so that the hydrochloric acid solution covers the sample.
[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: The control method of the tin plating equipment of the present invention, through sampling design along the width direction of the tin-plated plate, and further combined with a simple and easy-to-operate detinning method, uses inductively coupled plasma testing method to conduct batch testing and calculate the tin plating amount of each sample, thereby obtaining the tin plating amount distribution along the width direction of the tin-plated plate, effectively reflecting the edge effect in the tin plating process, and thus providing feedback on the working status of the tin plating equipment used in the tin plating process. This not only solves the problem of poor tin plating uniformity of the tin-plated plate, but also solves the technical problem that electrochemical methods cannot effectively peel off the tin oxide layer, metallic tin layer and tin-iron alloy layer. Moreover, the detinning solution used has a simple composition and does not require pH adjustment, which simplifies the experimental process and reduces costs. Based on the comparison results of the tin plating amount of each sample with the preset tin plating amount, the tin plating equipment can be adjusted in a targeted manner, so that the subsequently prepared tin-plated plates have excellent corrosion resistance and welding performance, meeting customer needs, and also providing data support for the development of new tin-plated products. Detailed Implementation
[0016] The technical solution of the present invention will be further described below with reference to specific embodiments, but the scope of protection is not limited to the description.
[0017] This invention provides a method for controlling a tin plating equipment, comprising the following steps performed sequentially: (1) Sampling The tinplate is divided into a first region and a second region along an axis of symmetry parallel to its length. Samples are then cut from the first region and the second region according to the sampling method.
[0018] Along the width direction of the tin-plated plate, the length of each sample gradually increases from the side edge of the tin-plated plate toward its midpoint along the width direction, and all samples have the same area.
[0019] That is, along the width direction of the tinplate, the sampling density gradually decreases from the side edge towards the midpoint of the width direction. Because the current linear density of the tin-plating anode in the side region of the steel plate is greater than that in the central region, the amount of tin plating in the side region after tin plating is much higher than that in the central region. This sampling method can effectively reflect the edge effect during the tin plating process, thus providing feedback on the working status of the tin plating equipment used in the tin plating process. Since the edge effect is less pronounced in the central region of the tinplate, the tin plating amount is more uniformly distributed, allowing for a reduction in the sample length along the width direction of the tinplate, thereby reducing workload. By controlling the area of all samples to be the same, the distribution of tin plating amount along the width direction of the tinplate can be scientifically reflected.
[0020] Specifically, the sampling method includes: establishing an X-axis with one side of the tin-plated plate as the origin, extending along the width of the tin-plated plate towards the other side; sequentially cutting samples from the origin along the X-axis towards the midpoint of the tin-plated plate along its width and numbering them in sequence, with the coordinates of the first and last ends of sample i along the X-axis being X... i 'and X i , where X i '=X i +ΔX i X1=0mm, ΔX i ≥ΔX i-1 1mm≤ΔX i ≤20mm; when i≤5, X i =X i-1 When i≥6, X i >X i-1 '.
[0021] Here, the first end of sample i# is the end of sample i# that is furthest from the origin of the coordinate system, and the last end of sample i# is the end of sample i# that is furthest from the origin of the coordinate system.
[0022] Both the first and second regions are sampled according to the sampling method described above, that is, the entire width of the tin-plated plate is sampled.
[0023] Along the width of the tinplate, samples are numbered starting from the side edges, with numbers 1# to 5# representing areas where edge effects are most significant during the tin plating process. By continuously sampling and measuring the tin plating amount in the side areas of the tinplate, the edge effects during the tin plating process can be reflected, thus providing feedback on the operating status of the tin plating equipment used. The central area of the tinplate, where edge effects are less pronounced and the tin plating amount is more uniform, is sampled at larger intervals, and the sample length along the width of the tinplate is reduced, thus decreasing workload.
[0024] Preferably, in this embodiment, the area of the sample is designed to be S=200mm². 2 This facilitates sampling and effectively provides feedback on the tin plating amount distribution along the width of the tin-plated plate.
[0025] Preferably, when i = 1~2, ΔX i =1mm; when i=3, ΔX i =2mm; when i=4~5, ΔX i =2~4mm.
[0026] Then the length of sample i# along the width direction of the tin-plated plate is ΔX. i The length of sample i# along the length direction of the tinplate is defined as the width b of sample i#. i Then S = ΔX i b i .
[0027] That is, along the width direction of the tin-plated plate, sampling is started from one side edge of the tin-plated plate. The length of the outermost 1# sample is ΔX1=1mm, and the width is b1=200mm, that is, X1=0mm, X1'=1mm. The length of sample #2 is ΔX2=1mm and the width is b2=200mm, that is, X2=1mm and X2'=2mm; The length of sample #3 is ΔX3=2mm, and the width is b3=100mm, that is, X3=2mm and X3'=4mm; The length of sample #4 is ΔX4=2mm, then the width is b4=100mm, that is, X4=4mm, X4'=6mm; If the length of sample #5 is ΔX5=2mm, then the width is b5=100mm, which means X5=6mm and X5'=8mm.
[0028] If the length of sample #4 is ΔX4=4mm, then the width is b4=50mm, that is, X4=4mm and X4'=8mm; If the length of sample #5 is ΔX5=4mm, then the width is b5=50mm, that is, X5=8mm and X5'=12mm.
[0029] In this way, by continuously sampling the side area of the tin-plated board over a short length and detecting the amount of tin plating, the distribution of tin plating in the side area of the tin-plated board can be obtained more accurately, thereby providing feedback on the working status of the tin-plating equipment used in the tin-plating process.
[0030] (2) The amount of tin plating was measured for each sample.
[0031] In the tin plating amount determination step, a beaker containing 60 mL of 30% hydrochloric acid solution is heated to 90°C. The sample is added to the beaker, and the heating temperature is maintained at 90°C until the surface of the tin-plated plate is completely dull or the solution in the beaker begins to turn yellow and produces a large number of bubbles. Heating is then stopped to avoid Fe from the steel plate dissolving into the solution and causing a matrix effect, which would affect the test results. The cooled solution is poured into a 100 mL volumetric flask, and 5 drops of concentrated hydrochloric acid are added to inhibit the hydrolysis of tin ions. Deionized water is then added to bring the volume to 100 mL. The tin ion concentration C in the volumetric flask is determined using inductively coupled plasma (ICP-PAP) testing. i And convert it into the tin plating amount ρ of each sample. i .
[0032] The chemical reaction equation for this process is as follows: 2HCl + Sn → H2 + SnCl2; 4HCl + Sn → 2H2 + SnCl4; 2HCl + SnO → H2O + SnCl2; 4HCl + SnO2 → 2H2O + SnCl4.
[0033] In this way, the tin layer of each sample can be stripped into the detinning solution, and then the tin ion concentration C in the corresponding volumetric flask of each sample can be determined by inductively coupled plasma (ICP-PAP) testing. i This is further converted into the tin plating amount ρ of each sample. i Thus, by using the tin plating amount data of all samples, the distribution of tin plating amount along the width direction of the tin-plated plate can be obtained, and the tin plating amount curve along the width direction of the tin-plated plate can be plotted.
[0034] This method for determining tin plating concentration is simple to operate, and the reaction endpoint is easy to determine. It can completely dissolve the tin in the tin oxide layer, metallic tin layer, and tin-iron alloy layer in the solution without the need for complex metal corrosion inhibitors or other additives, thus solving the technical problem that electrochemical methods cannot effectively peel off the tin oxide layer, metallic tin layer, and tin-iron alloy layer. Moreover, the solution used has a simple composition and does not require pH adjustment, which not only simplifies the experimental procedure but also reduces costs. In addition, the inductively coupled plasma testing method has the advantages of high testing precision, low cost, and ease of batch testing when measuring tin ion concentration.
[0035] Specifically, the tin plating amount ρ of each sample i Convert using the following formula: ρ i =50C i / S, where S is the area of the sample in mm. 2 C i The unit is mg / L; ρ i The unit is g / m 2 .
[0036] Preferably, before adding the sample to the beaker, the sample surface is wiped with alcohol to remove residual fingerprints, residual oil, etc., and reduce test errors.
[0037] Preferably, when adding the sample to the beaker, the sample is cut into small pieces and added to the beaker so that the hydrochloric acid solution covers the sample, so as to ensure that the sample is completely detinned and to avoid inaccurate test results.
[0038] (3) Tin plating equipment control steps.
[0039] The tin plating amount ρ of each sample i The tin plating amount ρ0 of the tin-plated plate is compared with the preset tin plating amount ρ0, and the tin plating equipment used in the tin plating process is adjusted according to the comparison result.
[0040] Specifically, the tin plating amount ρ of each sample when i≥6 i Compare with the preset tin plating amount ρ0; If i≥6, then ρ i If the fluctuation range exceeds the preset tin plating amount ρ0, then adjust the position of the tin plating anode or replace the tin plating anode.
[0041] The region of the tin-plated plate where the sample corresponding to i≥6 is located is the central region of the tin-plated plate that is not affected by edge effects. If the tin plating amount ρ of the sample is in this region... iIf the fluctuation range exceeds the preset tin plating amount ρ0, it indicates that the tin plating anode has shifted position or the tin ingot of the tin plating anode has been consumed. Therefore, it is necessary to adjust the position of the tin plating anode or replace the tin plating anode to ensure that the tin plating amount in the central area is within the fluctuation range of the preset tin plating amount ρ0 when the steel plate is subsequently tin-plated.
[0042] Furthermore, if i≥6, then ρ i If the fluctuation range exceeds the preset tin plating amount ρ0, the dispersion performance of the tin plating solution needs to be further checked, and whether the impurities in the tin plating solution exceed the standard. If the dispersion performance of the tin plating solution is unqualified, and / or if the impurities in the tin plating solution exceed the standard, the tin plating solution shall be replaced to avoid affecting the subsequent preparation of tin-plated plates.
[0043] Furthermore, if among samples 1-5, the difference in tin plating amount between the sample and the board is Δρ i If the value is greater than 2ρ0, then adjust the position of the anode edge cover to increase the shielding area of the anode edge cover on the tin-plated anode. Among them, the difference in tin plating amount between the sample and the board is Δρ i =ρ i -ρ0.
[0044] The areas of the tin-plated board corresponding to samples 1-5# are the edge areas of the tin-plated board that are significantly affected by edge effects. If the tin plating amount of a sample in this area differs from that of the board by Δρ... i If the amount exceeds twice the preset tin plating amount ρ0, it indicates that the shielding area of the anode edge cover on the tin-plated anode is too small, thus reducing the amount of tin plating in the edge area of the tin-plated plate.
[0045] In summary, this invention, through sampling design along the width of the tin-plated board and combining it with a simple and easy-to-operate detinning method, employs inductively coupled plasma (ICP) testing to conduct batch tests and calculate the tin plating amount of each sample. This allows for the determination of the tin plating amount distribution along the width of the tin-plated board, effectively reflecting the edge effect during the tin plating process and providing feedback on the working status of the tin plating equipment used in the tin plating process. This not only solves the problem of poor tin plating uniformity but also overcomes the technical challenge of effectively removing the tin oxide layer, metallic tin layer, and tin-iron alloy layer using electrochemical methods. Furthermore, the detinning solution used has a simple composition, requiring no pH adjustment, which simplifies the experimental process and reduces costs. Based on the comparison results of the tin plating amount of each sample with the preset tin plating amount, the tin plating equipment can be adjusted accordingly, resulting in tin-plated boards with excellent corrosion resistance and weldability, meeting customer needs. It also provides data support for the development of new tin-plated products.
[0046] The detailed descriptions listed above are merely specific descriptions of feasible embodiments of the present invention, and are not intended to limit the scope of protection of the present invention. All equivalent embodiments or modifications made without departing from the spirit of the present invention should be included within the scope of protection of the present invention.
[0047] The beneficial effects of the present invention will be further illustrated below through specific embodiments 1 and 2. Of course, these two embodiments are only a part of the many variations contained in the present invention, and not all of them.
[0048] Example 1 The tin-plated plate has a width of 832 mm, is tin-plated on both sides, and the preset tin plating amount ρ0 on one side is 1.1 g / m. 2 The allowable fluctuation range for the preset tin plating amount ρ0 of a single-sided tin layer is ±0.15 g / m. 2 .
[0049] (1) Sampling The tin-plated sheet was divided into a first region and a second region along an axis of symmetry parallel to its length. Samples were cut from the first and second regions according to the sampling method. The area of all samples was S = 200 mm². 2 .
[0050] Taking the first region as an example, the sampling method includes: taking the side edge of the tinplate located in the first region as the origin, establishing an X-axis along the width direction of the tinplate toward the other side; cutting samples sequentially from the origin along the X-axis toward the midpoint of the tinplate along the width direction and numbering them in order.
[0051] The second region was also sampled using the same sampling method as described above. In other words, the first and second regions were sampled symmetrically along the axis of symmetry parallel to the length of the tinplate.
[0052] In the first region, the coordinates X of the first and last ends of sample i# along the X-axis are... i '、X i The length of sample i# along the width direction of the tinplate is ΔX. i , and the width b of sample i# i The results are shown in Table 1.
[0053] In the second region, the coordinates X of the first and last ends of sample i# along the X-axis are... i '、X i The length of sample i# along the width direction of the tinplate is ΔX. i , and the width b of sample i# i The results are shown in Table 2.
[0054] (2) The amount of tin plating was measured for each sample.
[0055] In the tin plating amount determination step, a beaker containing 60 mL of 30% hydrochloric acid solution is heated to 90°C. The sample surface is first wiped with alcohol to remove residual fingerprints and oil. The sample is then cut into small pieces and added to the beaker so that the hydrochloric acid solution completely covers the sample. The heating temperature is maintained at 90°C until the tin-plated plate surface is completely dull or the solution in the beaker begins to turn yellow and produces a large number of bubbles. Heating is then stopped. The cooled solution is poured into a 100 mL volumetric flask, 5 drops of concentrated hydrochloric acid are added, and deionized water is added to bring the volume to 100 mL. The tin ion concentration C in the volumetric flask is determined using inductively coupled plasma (ICP-CPS) measurement. i And according to the formula ρ i =50C i / S is converted to obtain the tin plating amount ρ of the tin layer on one side of each sample. i The results are shown in Table 1 and Table 2, respectively.
[0056] Among them, C i The unit is mg / L; ρ i The unit is g / m 2 .
[0057] Table 1
[0058] Table 2
[0059] (3) Tin plating equipment control steps.
[0060] By comparison, when i≥6, the amount of tin plating on one side of all samples did not exceed the allowable fluctuation range of the preset amount of tin plating ρ0 on one side, indicating that the position of the tin-plated anode plate is reasonable, the working condition of the rectifier cabinet is good, the dispersion performance of the tin plating solution is stable, and the impurities in the tin plating solution meet the standards.
[0061] The amount of tin plating on one side of the tin layer of samples 1 to 3# showed significant fluctuations, especially sample 1#, which is the outermost sample. The difference in the amount of tin plating on one side of the tin layer was greater than 2ρ0. Furthermore, a bright edge appeared at the outermost edge of the tin-plated plate, which had a significant color difference from other parts. Therefore, it is necessary to adjust the position of the anode edge cover and increase the shielding area of the anode edge cover on the tin-plated anode to avoid affecting the solderability of the tin-plated plates prepared by continuing to use the tin-plating equipment.
[0062] Example 2 The tin-plated plate is 1000mm wide, double-sided tin-plated, and the preset tin plating amount ρ0 on one side is 2.8 g / m. 2 The allowable fluctuation range for the preset tin plating amount ρ0 of a single-sided tin layer is ±0.15 g / m. 2.
[0063] (1) Sampling The tin-plated sheet was divided into a first region and a second region along an axis of symmetry parallel to its length. Samples were cut from the first and second regions according to the sampling method. The area of all samples was S = 200 mm². 2 .
[0064] Taking the first region as an example, the sampling method includes: taking the side edge of the tinplate located in the first region as the origin, establishing an X-axis along the width direction of the tinplate toward the other side; cutting samples sequentially from the origin along the X-axis toward the midpoint of the tinplate along the width direction and numbering them in order.
[0065] The second region was also sampled using the same sampling method as described above. In other words, the first and second regions were sampled symmetrically along the axis of symmetry parallel to the length of the tinplate.
[0066] In the first region, the coordinates X of the first and last ends of sample i# along the X-axis are... i '、X i The length of sample i# along the width direction of the tinplate is ΔX. i , and the width b of sample i# i The results are shown in Table 3.
[0067] In the second region, the coordinates X of the first and last ends of sample i# along the X-axis are... i '、X i The length of sample i# along the width direction of the tinplate is ΔX. i , and the width b of sample i# i The results are shown in Table 4.
[0068] (2) The amount of tin plating was measured for each sample.
[0069] In the tin plating amount determination step, a beaker containing 60 mL of 30% hydrochloric acid solution is heated to 90°C. The sample surface is first wiped with alcohol to remove residual fingerprints and oil. The sample is then cut into small pieces and added to the beaker so that the hydrochloric acid solution completely covers the sample. The heating temperature is maintained at 90°C until the tin-plated plate surface is completely dull or the solution in the beaker begins to turn yellow and produces a large number of bubbles. Heating is then stopped. The cooled solution is poured into a 100 mL volumetric flask, 5 drops of concentrated hydrochloric acid are added, and deionized water is added to bring the volume to 100 mL. The tin ion concentration C in the volumetric flask is determined using inductively coupled plasma (ICP-CPS) measurement. i And according to the formula ρ i =50C i / S is converted to obtain the tin plating amount ρ of the tin layer on one side of each sample. iThe results are shown in Tables 3 and 4, respectively.
[0070] Among them, C i The unit is mg / L; ρ i The unit is g / m 2 .
[0071] Table 3
[0072] Table 4
[0073] (3) Tin plating equipment control steps.
[0074] By comparison, when i≥6, the amount of tin plating on one side of all samples did not exceed the allowable fluctuation range of the preset amount of tin plating on one side ρ0, indicating that the position of the tin plating anode plate is reasonable, the working condition of the rectifier cabinet is good, the dispersion performance of the tin plating solution is stable, the impurities in the tin plating solution meet the standards, and there is no need to adjust the position of the tin plating anode or replace the tin plating anode, nor is there a need to replace the tin plating solution.
[0075] The amount of tin plating on one side of the tin layer of samples 1 to 3 showed relatively obvious fluctuations, especially sample 1, which is the outermost sample. The difference in the amount of tin plating on one side of the tin layer with the board was Δρ1<2ρ0, indicating that the position of the anode edge cover was reasonable and the anode edge effect was well controlled, so there was no need to adjust the anode edge cover.
[0076] It should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This way of describing the specification is only for clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
[0077] The detailed descriptions listed above are merely specific descriptions of feasible embodiments of the present invention, and are not intended to limit the scope of protection of the present invention. All equivalent embodiments or modifications made without departing from the spirit of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method of regulating a tinning apparatus, characterized by, This includes sequential sampling, determination of the tin plating amount for each sample, and adjustment of the tin plating equipment. In the sampling step, the tinplate is divided into a first region and a second region along an axis of symmetry parallel to its length. Samples are cut from the first and second regions according to the sampling method. Along the width of the tinplate, the length of each sample gradually increases from the side edge towards the midpoint of the width direction, and all samples have the same area. The sampling method includes: establishing an X-axis with one side of the tinplate as the origin, extending along the width direction towards the other side; sequentially cutting samples from the origin along the X-axis towards the midpoint of the width direction of the tinplate and numbering them in sequence, with the coordinates of the first and last ends of sample i along the X-axis being X... i and X i ', where X i '=X i +ΔX i X1=0mm, ΔX i >ΔX i-1 1mm≤ΔX i ≤20mm; when i≤5, X i =X i-1 When i≥6, X i >X i-1 '; In the tin plating amount determination step, a beaker containing 60 mL of 30% hydrochloric acid solution is heated to 90°C. The sample is added to the beaker, and the heating temperature is maintained at 90°C until the surface of the tin-plated plate is completely dull or the solution in the beaker begins to turn yellow and produces a large number of bubbles. Heating is then stopped. The cooled solution is poured into a 100 mL volumetric flask, 5 drops of concentrated hydrochloric acid are added, and then deionized water is added to bring the volume to 100 mL. The tin ion concentration C in the volumetric flask is determined using inductively coupled plasma (ICP-CPS) measurement. i And convert it into the tin plating amount ρ of each sample. i ; In the tin plating equipment control step, the tin plating amount ρ of each sample is adjusted. i The tin plating process involves comparing the tin plating amount ρ0 with the preset tin plating amount of the tin-plated plate, and adjusting the tin plating equipment used in the tin plating process based on the comparison result. This includes: If the tin plating amount p of each sample where i is 6 or more is i If the tin plating amount p of each sample where i is 6 or more is outside the fluctuation range of the preset tin plating amount p0, the position of the tin plating anode is adjusted or the tin plating anode is replaced. If the tin plating amount of a sample in the 1~5# samples is different from the plate difference Δρ i 2ρ0, the position of the anode edge cover is adjusted to increase the shielding area of the anode edge cover to the tin plating anode; wherein the tin plating amount of the sample in the 1~5# samples is different from the plate difference Δρ i =ρ i -ρ0.
2. The control method for tin plating equipment according to claim 1, characterized in that, If the tin plating amount p of each sample where i is 6 or more is i If the tin plating amount p of each sample where i is 6 or more is outside the fluctuation range of the preset tin plating amount p0, the dispersion performance of the tin plating solution is checked, and whether the impurities in the tin plating solution are over the standard is detected. If the dispersion performance of the tin plating solution is unqualified, and / or the impurities in the tin plating solution exceed the standard, the tin plating solution shall be replaced.
3. The control method for tin plating equipment according to claim 1, characterized in that, The area of the sample was 200 mm 2 .
4. The control method for tin plating equipment according to claim 1, characterized in that, In the tin plating amount determination step, the sample surface is wiped with alcohol before adding the sample to the beaker.
5. The control method for tin plating equipment according to claim 1, characterized in that, In the tin plating amount determination step, when adding the sample to the beaker, the sample is cut into small pieces and added to the beaker so that the hydrochloric acid solution covers the sample.
Citation Information
Patent Citations
High-tin tinned plate edge quality control method
CN107740173A
River sediment sampling method
CN115950679A