A method for preparing Co-CuO (Ov) single-atom catalyst for treating water pollution

The preparation of Co-CuO(Ov) single-atom catalysts through redox-driven hydrolysis method has solved the problems of difficult separation of existing catalysts and poor catalytic effects, achieved efficient removal of difficult-to-degrade organic pollutants in water, and provided stability and Efficient water treatment solution.

CN116726929BActive Publication Date: 2024-11-12SHENYANG INSTITUTE OF CHEMICAL TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310581497.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-12
Estimated Expiration
2043-05-23

AI Technical Summary

Technical Problem

The existing homogeneous and heterogeneous catalysts have difficulties in separation, metal ion contamination and unsatisfactory catalytic effects in water treatment, making it difficult to effectively remove difficult-to-degrade organic pollutants in water.

Method used

Co-CuO(Ov) single atom catalyst was prepared by redox-driven hydrolysis method, and single atom Co was fixed using the oxygen vacancies of CuO to improve the load and catalytic performance of metal atoms. Co-CuO(Ov) was prepared by two-step calcination. It is also combined with the potassium perhydrogen sulfate (PMS) system for contaminated water treatment.

Benefits of technology

It has achieved efficient removal of difficult-to-degrade organic pollutants in water, easy to recover catalysts, less metal ions leaching, excellent catalytic activity and stability, and can remove specific pollutants 100% in a short period of time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

A method for preparing a Co-CuO (Ov) single-atom catalyst for treating water pollution relates to a method for treating polluted water. The invention utilizes the oxygen vacancies (O v )Increasing the single-atom Co loading of Co‑CuO(O v ) single atom catalyst preparation method and application thereof. The present invention is based on a single atom catalyst having oxygen vacancies (O v ) was used as the support of single-atom catalysts, and single-atom Co was loaded onto CuO(O) by redox-driven hydrolysis. v ) to prepare Co‑CuO(O v ) single-atom catalyst. The prepared catalyst can efficiently remove refractory organic pollutants in water, achieving the purpose of harmlessness and protecting the water environment. Moreover, the catalyst is easy to recycle, has little metal ion leaching, and has excellent catalytic activity and stability. Under certain conditions, Co‑CuO(O v ) / PMS system can 100% remove rhodamine B with a concentration of 10-100 mg / L in 5 minutes, and 100% remove tetracycline with a concentration of 10-50 mg / L in 15 minutes. It can effectively remove refractory organic pollutants in water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for treating polluted water, in particular to a method for preparing a Co-CuO (Ov) single-atom catalyst for treating water pollution. Background Art

[0002] Water is the source of life and the foundation of human survival and development. Although the total amount of water in my country is large, it is also suffering from varying degrees of pollution, and there is very little water available for human use. Among them, refractory organic pollutants are an important cause of water pollution. Therefore, how to effectively remove refractory organic pollutants in water is an issue that researchers are paying close attention to. At present, sulfate free radical advanced oxidation technology is widely used in the field of water treatment. It is mainly through the use of various catalysts to activate persulfate, so that the OO bond in it breaks to produce highly oxidizing sulfate free radicals, hydroxyl radicals and other active oxygen species. These active oxygen species will further react with organic pollutants to decompose them and convert them into non-toxic intermediates, water and carbon dioxide. Catalysts are divided into homogeneous catalysts (transition metal ions, such as Fe 2+ 、Co 2+ , Cu 2+ There are two categories of catalysts: homogeneous catalysts (metal oxides, carbon-based materials, etc.) and heterogeneous catalysts (metal oxides, carbon-based materials, etc.). However, homogeneous and heterogeneous catalysts have certain defects, such as homogeneous catalysts are not easy to separate and easily cause metal ion pollution; heterogeneous catalysts have unsatisfactory catalytic effects, etc.

[0003] Therefore, developing a catalyst that has the advantages of both homogeneous and heterogeneous catalysts and can make up for their shortcomings is an urgent problem to be solved. Recently emerging single atom catalysts (SACs) have high catalytic efficiency, easy recovery, high atom utilization, and a wide pH application range, and are considered to be a bridge between homogeneous and heterogeneous catalysis. However, single metal atoms are very unstable and easily aggregated into clusters or nanoparticles. Therefore, choosing a suitable carrier is crucial to stabilize single metal atoms and inhibit aggregation. The presence of cationic defect sites in metal oxides is very beneficial to stabilizing single metal atoms and increasing the loading amount of metal atoms, making them ideal carriers for single atom catalysts. It can be seen that proposing a SACs with metal oxides with defect sites as single metal atom carriers has important practical significance for the development of water environment remediation. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a Co-CuO(Ov) single-atom catalyst for treating water pollution. The present invention adopts a redox-driven hydrolysis method to prepare Co-CuO(Ov) with a high Co atom loading. v), the prepared catalyst can efficiently remove the refractory organic pollutants in water, achieving the purpose of harmlessness and protecting the water environment. Moreover, the catalyst is easy to recycle, has little metal ion leaching, and has excellent catalytic activity and stability.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] A method for preparing a Co-CuO (Ov) single-atom catalyst for treating water pollution, wherein the catalyst preparation method utilizes oxygen vacancies (O v )Preparation of Co-CuO(O) loaded with single-atom Co v ) single atom catalyst, the steps are as follows:

[0007] Metal oxide CuO(O v ) as a carrier of single-atom Co, using the O v Fixing single-atom Co, increasing the loading of single-atom Co, reducing the aggregation of Co atoms and improving the catalytic performance of the catalyst; Cu(NO3)2·3H2O and Co(NO3)2·6H2O as CuO(O v ) and single-atom Co precursors; first, the pH of 0.5-0.9 mol / L Cu(NO3)2·3H2O solution was adjusted to 9-14 with 1-5 mol / L NaOH solution, and stirred for 1-5 h in a 60-100 °C water bath; after washing with ethanol and deionized water, the solution was calcined at 200-600 °C for 1-5 h to obtain CuO(O v ); then the single-atom Co is loaded onto CuO(O v ) on; 0.2-0.7 g CuO(O v ) was dissolved in 50-120 mL of deionized water, and then 1-5 mL of Co(NO3)2·6H2O solution (0.1-0.4 g / mL) was added and stirred evenly; the diluted H2O2 solution was slowly added to the mixed solution and stirred continuously until no obvious bubbles were generated; finally, it was washed with deionized water and calcined at 250-650 ℃ for 1-5 h to obtain Co-CuO(O v ).

[0008] The single-atom catalyst is prepared by two-step calcination, wherein Cu(NO3)2·3H2O is used as a precursor and CuO(Ov) is prepared by one-step calcination. v ), doped with single-atom Co and then subjected to secondary calcination.

[0009] The method for preparing a Co-CuO(Ov) single-atom catalyst for treating water pollution, wherein the prepared Co-CuO(Ov) v ) single-atom catalyst for treating polluted water, using potassium persulfate (PMS) as an oxidant and Co-CuO(O v ) as a catalyst to establish a water pollution treatment system.

[0010] The advantages and effects of the present invention are:

[0011] 1. The present invention adopts a redox driven hydrolysis method to prepare Co-CuO (O v ), the prepared catalyst can effectively remove the refractory organic pollutants in water, achieving the purpose of harmlessness and protecting the water environment. Moreover, the catalyst is easy to recycle, has little metal ion leaching, and has excellent catalytic activity and stability. Under certain conditions, Co-CuO(O v ) / PMS system can remove 100% of rhodamine B with a concentration of 10-100 mg / L in 5 minutes; and can remove 100% of tetracycline with a concentration of 10-50 mg / L in 15 minutes. In this catalytic system, free radical pathways (sulfate radicals, hydroxyl radicals) and non-free radical pathways (electron transfer, singlet oxygen) jointly lead to the removal of pollutants. Among them, electron transfer is the main pathway for pollutant removal, while sulfate radicals, hydroxyl radicals and singlet oxygen also play a certain role in the removal of pollutants.

[0012] 2. The present invention solves the problems of low metal atom loading, poor activity and limited pollutant removal rate in SACs, and provides a method for preparing SACs with high metal atom loading, so that they exhibit better catalytic performance and can efficiently remove difficult-to-degrade organic pollutants in water. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 is Co-CuO(O v ) SEM and HRTEM images of single atom catalysts;

[0014] Figure 2 is Co-CuO(O v ) The degradation effect diagram of rhodamine B (RhB), tetracycline (TC), methylene blue (MB), and phenol;

[0015] Figure 3 is Co-CuO(O v )Stability effect diagram. Implementation

[0016] The present invention is described in detail below with reference to the embodiments.

[0017] The present invention utilizes the oxygen vacancies (O v )Increasing the single-atom Co loading of Co-CuO(O v ) The preparation method of the single atom catalyst is as follows:

[0018] 1) Use NaOH solution to adjust the pH of Cu(NO3)2·3H2O solution. The concentration of NaOH solution is 1-5 mol / L, the concentration of Cu(NO3)2·3H2O solution is 0.5-0.9 mol / L, and the pH is 9-14.

[0019] 2) Place the solution in step 1) in a water bath and stir. The water bath is heated to 60-100°C and stirred for 1-5 h.

[0020] 3) The black solid treated in step 2) is placed in a centrifuge and washed with ethanol and deionized water. The centrifuge speed is 8000 r / min and the ethanol concentration is 95%.

[0021] 4) The washed solid is placed in a muffle furnace and calcined at a certain heating rate; the calcination temperature is 200-600°C, the calcination time is 1-5 h, and the heating rate is 2-10°C / min.

[0022] 5) The solid obtained in step 4) is dispersed in deionized water. The solid mass is 0.2-0.7 g, and the volume of deionized water is 50-120 mL.

[0023] 6) Add Co(NO3)2·6H2O solution and stir evenly. The volume of Co(NO3)2·6H2O solution is 1-5 mL, and the concentration is 0.1-0.4 g / mL.

[0024] 7) Slowly add diluted H2O2 solution and stir continuously until no obvious bubbles are generated. The concentration of diluted H2O2 solution is 1-10 wt.%.

[0025] 8) Wash with deionized water and place in a muffle furnace for calcination at a certain heating rate. The calcination temperature is 250-650℃, the calcination time is 1-5 h, and the heating rate is 2-10℃ / min.

[0026] The following Co-CuO(O v ) was used as a catalyst to carry out degradation tests on wastewater containing difficult-to-degrade organic pollutants.

[0027] Example 1: 0.02 g Co-CuO(O v) was added to a 100 mL volume of 20 mg / L RhB solution and 100-200 μL of PMS (0.5 mol / L) was added to start the catalytic reaction. After the addition of PMS, 100% of RhB was removed within 5 min.

[0028] Example 2: 0.02 g Co-CuO(O v ) was added to a 100 mL TC solution with a concentration of 20 mg / L and 100-200 μL of PMS (0.5 mol / L) was added to start the catalytic reaction. After the addition of PMS, 100% of TC was removed in 15 min.

[0029] Example 3: 0.02 g Co-CuO(O v ) was added to a 100 mL, 20 mg / L MB solution and 100-200 μL of PMS (0.5 mol / L) was added to start the catalytic reaction. After the addition of PMS, 100% of MB was removed within 10 min.

[0030] Example 4: 0.02 g Co-CuO(O v ) was added to a 100 mL phenol solution with a concentration of 20 mg / L and 100-200 μL of PMS (0.5 mol / L) was added to start the catalytic reaction. After adding PMS, more than 98% of phenol could be removed in 15 minutes.

Claims

1. A Co-CuO(O) for treating water pollution v ) A method for preparing a single atom catalyst, characterized in that: Metal oxide CuO(O v ) as a single-atom Co carrier, using the oxygen vacancies O on the CuO surface v Fixed single atom Co, the catalyst preparation steps are as follows: 1) Use NaOH solution to adjust the pH of Cu(NO3)2·3H2O solution. The concentration of NaOH solution is 1-5 mol / L, the concentration of Cu(NO3)2·3H2O solution is 0.5-0.9 mol / L, and the pH is 9-14. 2) Place the solution in step 1) in a water bath and stir; the water bath is heated to 60-100°C and stirred for 1-5 h; 3) The black solid treated in step 2) is placed in a centrifuge and washed with ethanol and deionized water; the centrifuge speed is 8000 r / min, and the ethanol concentration is 95%; 4) The washed solid is placed in a muffle furnace and calcined at a certain heating rate; the calcination temperature is 200-600°C, the calcination time is 1-5 h, and the heating rate is 2-10°C / min; 5) The solid obtained in step 4) is dispersed in deionized water; the solid mass is 0.2-0.7 g, and the deionized water volume is 50-120 mL; 6) Add Co(NO3)2·6H2O solution and stir evenly; the volume of Co(NO3)2·6H2O solution is 1-5 mL, and the concentration is 0.1-0.4 g / mL; 7) Slowly add diluted H2O2 solution and keep stirring until no obvious bubbles are generated; the concentration of the diluted H2O2 solution is 1-10wt.%; 8) Wash the product obtained in step 7) with deionized water and place it in a muffle furnace for calcination at a certain heating rate; the calcination temperature is 250-650°C, the calcination time is 1-5h, and the heating rate is 2-10°C / min.

2. A water-polluted Co-CuO(O) prepared by the preparation method according to claim 1 v ) Application of a single atom catalyst, characterized in that 0.02 g Co-CuO(O v ) was added to a 100 mL RhB solution with a concentration of 20 mg / L and 100-200 μL of 0.5 mol / L PMS was added to start the catalytic reaction; after the addition of PMS, 100% of RhB could be removed within 5 min.

3. A water-polluted Co-CuO(O) prepared by the preparation method according to claim 1 v ) Application of a single atom catalyst, characterized in that 0.02 g Co-CuO(O v ) was added to a 100 mL tetracycline TC solution with a concentration of 20 mg / L and 100-200 μL of 0.5 mol / L PMS was added to start the catalytic reaction; after the addition of PMS, 100% of the tetracycline TC could be removed in 15 min.

4. A water-polluted Co-CuO(O) prepared by the preparation method according to claim 1 v ) Application of a single atom catalyst, characterized in that 0.02 g Co-CuO(O v ) was added to a 100 mL methylene blue MB solution with a concentration of 20 mg / L and 100-200 μL of 0.5 mol / L PMS was added to start the catalytic reaction; after the addition of PMS, 100% of the methylene blue MB could be removed in 10 min.

5. A water-polluted Co-CuO(O) prepared by the preparation method according to claim 1 v ) Application of a single atom catalyst, characterized in that 0.02 g Co-CuO(O v ) was added to a 100 mL phenol solution with a concentration of 20 mg / L and 100-200 μL of 0.5 mol / L PMS was added to start the catalytic reaction; after the addition of PMS, 98% of the phenol could be removed in 15 min.