A quartz crucible and preparation method thereof

By adjusting the vacuum degree and current firing method, combined with reasonable quartz sand formula and mold speed, the bubble problem in the inner wall of the quartz crucible is solved, the density and pressure resistance of the crucible are improved, and high-quality quartz crucible preparation is achieved.

CN116730596BActive Publication Date: 2024-12-06JIANGSU XINYIYANG HIGH TECH MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310768498.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-28
Publication Date
2024-12-06
Estimated Expiration
2043-06-28

AI Technical Summary

Technical Problem

During the vacuum arc preparation process of existing quartz crucibles, there are still a small number of bubbles on the inner wall, which affects the volume density and pressure resistance of the crucible, and lacks mature processing technology.

Method used

By adjusting the melting vacuum degree and arcing current, a quartz crucible is fired in an inert atmosphere, combining reasonable quartz sand raw material formula and mold speed control, ensuring that there are no bubbles in the inner layer and uniform bubbles in the outer layer, reducing the porosity. Improve bulk density and compressive strength.

Benefits of technology

The obtained quartz crucible has high volume density, low porosity and high pressure resistance, ensuring that there are no bubbles in the inner layer and uniform bubbles in the outer layer, improving the yield and overall performance of the crucible.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present application relates to the technical field of crucibles, and specifically discloses a quartz crucible and a preparation method thereof. The volume density of the quartz crucible provided in the present application is ≥1.72 g / cm 3 , apparent porosity ≤13.9%, compressive strength ≥52MPa. The above quartz crucible is obtained by a firing process under an inert atmosphere: the firing process includes the following steps: first arc melting, second arc melting and stable firing. The quartz crucible obtained by the above preparation method has a lower apparent porosity, a higher bulk density, and excellent compressive strength performance of the quartz crucible.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of crucibles, and in particular to a quartz crucible and a preparation method thereof. Background Art

[0002] Silicon single crystal is one of the most important raw materials for making silicon-based semiconductor materials and solar cells. Silicon single crystal is mainly made by placing polycrystalline silicon raw materials in a quartz crucible through the Czochralski method. The quartz crucible is generally a multi-layer structure, and the inner wall is a transparent layer without bubbles. The inner wall of the quartz crucible is in contact with the silicon melt. If there are bubbles on the inner wall, the bubbles will break due to the erosion of the silicon melt at high temperature. If the broken fragments are dissolved in the silicon melt, it will affect the yield and quality of the silicon single crystal; the outer wall is a non-transparent layer with a large amount of bubbles. The outer layer needs to evenly scatter the heat from the heater, so bubbles of appropriate number and size are required to evenly heat the silicon melt.

[0003] Quartz crucibles are generally made by vacuum arc method. Although the vacuum environment is conducive to the discharge of bubbles from the inner wall to the outer wall, there are still a small number of bubbles on the inner wall of the quartz crucible prepared by this method. Therefore, the crucible preparation process, especially the firing process that affects the distribution of bubbles in each layer of the crucible, has extremely high requirements, but there is no mature and effective treatment process. Summary of the invention

[0004] In order to obtain a quartz crucible with higher volume density and lower apparent porosity, so that the inner layer of the quartz crucible is free of bubbles and the outer layer of bubbles is uniform, so as to prepare a high-quality quartz crucible, the present application provides a quartz crucible and a preparation method thereof.

[0005] In a first aspect, the present application provides a quartz crucible, wherein the volume density of the quartz crucible is ≥1.72 g / cm 3 , apparent porosity ≤13.9%, compressive strength ≥52MPa.

[0006] Preferably, the volume density of the quartz crucible is ≥1.91 g / cm 3 , apparent porosity ≤11.7%, compressive strength ≥60MPa.

[0007] Preferably, the quartz crucible comprises the following components in parts by weight: 8-15 parts of inner layer material, 65-75 parts of middle layer material and 20-28 parts of outer layer material;

[0008] The inner layer material comprises 70-100 μm quartz sand, 100-300 μm quartz sand and 300-350 μm quartz sand in a weight ratio of (78-85): (30-45): (1-3);

[0009] The middle layer material comprises 70-100 μm quartz sand, 100-300 μm quartz sand and 300-350 μm quartz sand in a weight ratio of (70-78): (16-22): (24-30);

[0010] The outer layer material comprises 70-100 μm quartz sand, 100-300 μm quartz sand and 300-350 μm quartz sand in a weight ratio of (70-78): (10-16): (10-16).

[0011] After test analysis, it is known that when the formula of quartz sand raw materials is the above scheme, the volume density and compressive strength of the quartz crucible can be further improved, and the apparent porosity of the quartz crucible can be reduced. The inner layer of quartz sand has a relatively small particle size and a relatively high purity, which can better reduce the content of tiny bubbles in the transparent layer. The quartz sand in the middle and outer layers has a relatively large particle size and a relatively low purity, which can reduce the cost of raw materials while ensuring product quality, and at the same time improve the insulation effect of the outer bubble layer of the crucible.

[0012] Preferably, the size of the quartz crucible is 32-36 inches;

[0013] When the size of the quartz crucible is 32 inches, the total amount of quartz sand is 85-95 kg, and the specific specifications of the quartz crucible are height 570-630 mm, outer diameter 805-856 mm, and thickness 13.5-14 mm;

[0014] When the size of the quartz crucible is 36 inches, the total amount of quartz sand used is 105-115 kg, and the specific specifications of the quartz crucible are a height of 630-680 mm, an outer diameter of 905-948 mm, and a thickness of 13.5-16 mm.

[0015] By using the preparation method provided in the present application, the obtained quartz crucible has no bubbles in the inner layer and uniform bubbles in the outer layer, so that the quartz crucible has a lower apparent porosity, a higher volume density, and a stronger compressive strength.

[0016] In a second aspect, the present application provides a method for preparing the above-mentioned quartz crucible, wherein the quartz crucible is obtained by a firing process, and the firing process comprises the following steps:

[0017] Under the conditions of inert atmosphere and rotation speed of 60-80rpm, the quartz crucible blank is continuously subjected to the following steps:

[0018] First arc melting: In the time period of 0-(25-35)s, the first vacuum degree is controlled to be 0.01-0.02Mpa, and the arc current is uniformly increased from zero to the first arc current of 2000-2800A;

[0019] Second arc melting: in the time period of (25-35)-(150-210) s, the second vacuum degree is controlled to be 0.09-0.1Mpa, and the arc current is uniformly increased from the first arc current to the second arc current of 4600-5000A;

[0020] Stable firing: the second vacuum degree and the second arc starting current are maintained unchanged, and stable firing is performed for 15-18 minutes.

[0021] The inventor of the present application has found that during the vacuum arc firing process, by continuously changing the melting vacuum and the arc starting current within a certain period of time, the crucible raw material can be heated evenly, the melting speed is consistent, and the generation of bubbles in the quartz crucible is reduced. Therefore, using the preparation method provided by the present application, the inner layer of the obtained quartz crucible is free of bubbles, and the outer layer of bubbles is uniform, thereby making the quartz crucible have a lower apparent porosity, a higher volume density, and a stronger compressive strength.

[0022] In a specific embodiment, during the firing process, the rotation speed of the melting mold can be 60 rpm, 65 rpm, 70 rpm, 75 rpm, or 80 rpm.

[0023] In some specific embodiments, during the firing process, the rotation speed of the melting mold can also be 60-65rpm, 60-70rpm, 60-75rpm, 65-70rpm, 65-75rpm, 65-80rpm, 70-75rpm, 70-80rpm, 75-80rpm.

[0024] Through experimental analysis, it can be known that during the firing process of the quartz crucible, when the rotation speed is controlled within the above range, the volume density and compressive strength of the quartz crucible can be further improved, and the apparent porosity of the quartz crucible can be reduced.

[0025] Preferably, the firing process is implemented using an arc melting furnace, which includes a graphite electrode, a heat shield, an air blowing device, a compressed air nozzle, and an exhaust pipe.

[0026] Preferably, during the stable firing process, the oxide layer is removed every 2-3 minutes. The specific steps are: the graphite electrode is moved out of the melting mold, the oxide layer on the graphite electrode is removed by the blowing device, and then the graphite electrode is moved down to the original position in the melting mold, and then the stable firing is performed; the oxide layer removal process is controlled within 3 minutes.

[0027] The present invention lowers the graphite electrode into the melting mold before starting the ignition and arcing; and during the stable firing process, the graphite electrode is moved out of the mold to remove the oxide layer on the graphite electrode, which can effectively ensure that the crucible raw material is heated more evenly, so that the melting speed of the quartz raw material remains consistent, thereby reducing the generation of bubbles and black spots in the quartz crucible and improving the yield of the quartz crucible product.

[0028] Preferably, a heat shield is provided in the melting mold; before the first arc melting, the heat shield is arranged to be located 130-150 m above the melting mold.

[0029] Preferably, during the stable firing process, when the oxidation layer is removed every 2-3 minutes, the position of the heat shield needs to be adjusted. The specific steps are: move the heat shield up to 160-180m above the melting mold, and then move the graphite electrode out of the melting mold. After the oxidation layer removal operation is completed, move the heat shield and the graphite electrode down to their original positions, and then perform the stable firing. The adjustment process is controlled within 3 minutes.

[0030] During the process of removing the oxide layer, the present application reasonably adjusts the position of the heat shield plate, thereby preventing the heat shield plate from deformation, leakage, burns, etc. due to long-term close proximity to the graphite electrode, thereby causing the quartz crucible to be of unqualified quality.

[0031] Preferably, the inert atmosphere is one or a mixture of helium, argon and nitrogen.

[0032] Preferably, the preparation method of the quartz crucible blank is: rotating the quartz sand raw material at a rotation speed of 80-100 rpm to obtain the quartz crucible blank.

[0033] Furthermore, the preparation method of the quartz crucible blank is: the quartz sand raw material is rotationally molded at a rotation speed of 85-95 rpm to obtain the quartz crucible blank.

[0034] In a specific embodiment, in the method for preparing a crucible blank, the rotation speed of the melting mold can be 80 rpm, 85 rpm, 90 rpm, 95 rpm, or 100 rpm.

[0035] In some specific embodiments, in the method for preparing the crucible blank, the rotation speed of the melting mold can also be 80-85 rpm, 80-90 rpm, 80-95 rpm, 85-90 rpm, 85-100 rpm, 90-95 rpm, 90-100 rpm, or 95-100 rpm.

[0036] The present application can shape the quartz sand raw material under the optimal centrifugal force by selecting the appropriate mold rotation speed, thereby avoiding the loss of raw material on the straight wall of the mold or the throwing out of the raw material at the bottom of the mold due to excessive or insufficient centrifugal force, thereby effectively improving the uniformity of the raw material during the quartz crucible molding process, thereby preventing the defect of extremely increased bubbles in the subsequent melting process caused by uneven raw materials in the quartz crucible blank.

[0037] Through experimental analysis, it can be known that in the method for preparing the quartz crucible blank, when the rotation speed of the melting mold is controlled within the above range, the volume density and compressive strength of the quartz crucible can be further improved, and the apparent porosity of the quartz crucible can be reduced.

[0038] Furthermore, the method further comprises the following steps: cooling, demoulding, sandblasting and cutting the quartz crucible blank to obtain a quartz crucible finished product.

[0039] In summary, the technical solution of this application has the following effects:

[0040] In the vacuum arc firing process of the present application, by continuously changing the melting vacuum degree and the arc starting current within a certain period of time, the crucible raw material can be heated evenly, the melting speed is consistent, and the generation of bubbles in the quartz crucible is reduced, thereby making the quartz crucible have a lower apparent porosity, a higher volume density, and a stronger compressive strength.

[0041] In the present application, during the stable firing process, the graphite electrode is moved out of the mold, the oxide layer on the graphite electrode is removed, and the position of the heat shield is changed, which can further ensure that the crucible raw material is heated more evenly, thereby improving the performance and yield rate of the quartz crucible product.

[0042] The present application further improves the performance of the quartz crucible by screening suitable quartz sand raw materials, molding at a suitable mold rotation speed, and then coordinating with a corresponding firing method. DETAILED DESCRIPTION

[0043] The present application is further described in detail below in conjunction with examples, comparative examples and performance testing experiments. These examples should not be construed as limiting the scope of protection claimed in the present application.

[0044] The arc melting furnace (model 28-46 inch quartz melting furnace) used in the embodiment was purchased from Jiangxi Zhanxuan Optoelectronics Technology Co., Ltd. The arc melting furnace includes a melting mold, a graphite electrode, a heat shield, a blowing device, a compressed air nozzle, an exhaust pipe and other components. The heat shield and the graphite electrode are arranged in coordination; during the firing process of the quartz crucible, the heat shield and the graphite electrode are automatically raised and lowered according to the control requirements during the firing process.

[0045] Example

[0046] Example 1

[0047] This embodiment provides a quartz crucible.

[0048] The preparation method of the quartz crucible in this embodiment specifically includes the following steps:

[0049] S1: Adding material

[0050] Ingredients: The quartz sand raw materials include 10kg inner layer material, 70kg middle layer material and 25kg outer layer material; the raw materials at different positions are packed in barrels;

[0051] The inner layer material is 80μm quartz sand, 200μm quartz sand and 320μm quartz sand in a weight ratio of 80:33:2; the middle layer material is 80μm quartz sand, 200μm quartz sand and 320μm quartz sand in a weight ratio of 74:19:27; the outer layer material is 80μm quartz sand, 200μm quartz sand and 320μm quartz sand in a weight ratio of 74:13:13.

[0052] Start the melting mold and make it rotate; then the loader performs each step of the loading operation according to the loading operation technical specifications specified in JC∕T 1048-2018, and adds the outer layer material, the middle layer material and the inner layer material into the melting mold in batches. After each layer of raw materials is loaded, the corresponding forming rods need to be used for forming. Under the condition of a rotation speed of 90rpm, the rotational forming is carried out, and the quartz sand is formed into a crucible blank by the centrifugal force generated by the rotation of the mold;

[0053] Among them, the following points should be noted during the loading operation: when loading the outer layer of material, use the outer forming rod to shape the straight wall evenly, the R corner cannot be excessive, and the upper mouth cannot be scraped too thin to avoid scraping the secondary material; when loading the middle layer of material, use the middle forming rod to shape the straight wall evenly, and it is strictly forbidden to scrape the R corner of the middle layer material to the outer wall; when loading the inner layer of material, use the inner forming rod to shape the straight wall evenly, hold the inner forming rod straight and tightly, and it is strictly forbidden to shake the inner layer of material drastically, and the R corner should not be excessive to avoid flying material at the bottom causing black spots in the R corner interlayer.

[0054] S2: Firing: The rotation speed of the melting mold is maintained at 70 rpm, and the high-temperature arc is released through the graphite electrode to melt the quartz sand. During this process, the inert atmosphere N is maintained in the melting furnace. 2 ; The specific details are as follows:

[0055] The melting mold with the crucible blank is kept at a rotation speed of 70 rpm, moved into the arc melting furnace, the graphite electrode is lowered to the middle position of the melting mold, and the heat shield is kept 150m above the melting mold, in the shielding and heat preservation position, and arc melting is started;

[0056] First arc melting: in the time period of 0-30s, the first vacuum degree is controlled to be 0.015Mpa, and the arc current is uniformly increased from zero to the first arc current of 2600A;

[0057] Second arc melting: in the time period of 30-180s, the second vacuum degree is controlled to be 0.095Mpa, and the arc current is uniformly increased from the first arc current of 2600A to the second arc current of 4800A;

[0058] Stable firing: Maintain the second vacuum degree and the second arc starting current unchanged, and perform stable firing for 18 minutes. During the stable firing process, remove the oxide layer every 3 minutes. The specific steps are: move the heat shield plate up to 170m above the melting mold, and move the graphite electrode out of the melting mold, and use the blowing device of the arc melting furnace to remove the oxide layer on the graphite electrode; then move the heat shield plate and the graphite electrode down to their original positions, and the oxide layer removal process is controlled within 3 minutes;

[0059] Turn off the power supply of the graphite electrode, keep the heat shield in the reset and heat preservation position, and keep warm for 3 minutes. Then remove the heat shield and the graphite electrode, end the firing, and obtain the quartz crucible blank.

[0060] S3: post-processing such as cooling, demoulding, sandblasting and cutting

[0061] The melting mold and the quartz crucible blank are allowed to cool naturally while maintaining a rotation speed of 70 rpm; then, the quartz crucible is separated from the mold under the action of high-pressure airflow and knocking vibration;

[0062] After a preliminary inspection of the quartz crucible to ensure that there are no defects such as black spots, bubbles, cracks, etc., it enters the subsequent sandblasting and cutting operations; the quartz crucible is further tested for various indicators, and if it is qualified, it is cleaned, dried, packaged, etc., to obtain a 36-inch quartz crucible finished product (specific specifications are height 630mm, outer diameter 943mm, thickness 15.5mm).

[0063] Example 2

[0064] This embodiment provides a quartz crucible.

[0065] The difference between this embodiment and embodiment 1 is that the rotation speed of the melting mold is 60 rpm.

[0066] Example 3

[0067] This embodiment provides a quartz crucible.

[0068] The difference between this embodiment and embodiment 1 is that the rotation speed of the melting mold is 80 rpm.

[0069] Example 4

[0070] This embodiment provides a quartz crucible.

[0071] The difference between this embodiment and embodiment 1 is that: no oxidation layer removal process is performed during the firing process of step S2, and the specific steps are as follows:

[0072] S2: Firing: The rotation speed of the melting mold is maintained at 70 rpm, and the high-temperature arc is released through the graphite electrode to melt the quartz sand. During this process, the inert atmosphere N is maintained in the melting furnace. 2 ; The specific details are as follows:

[0073] The melting mold with the crucible blank is kept at a rotation speed of 70 rpm, moved into the arc melting furnace, the graphite electrode is lowered to the middle position of the melting mold, and the heat shield is kept 150m above the melting mold, in the shielding and heat preservation position, and arc melting is started;

[0074] First arc melting: in the time period of 0-30s, the first vacuum degree is controlled to be 0.015Mpa, and the arc current is uniformly increased from zero to the first arc current of 2600A;

[0075] Second arc melting: in the time period of 30-180s, the second vacuum degree is controlled to be 0.095Mpa, and the arc current is uniformly increased from the first arc current of 2600A to the second arc current of 4800A;

[0076] Stable firing: Maintain the second vacuum degree and the second arc starting current unchanged, and perform stable firing for 18 minutes. During the stable firing process, adjust the position of the heat shield every 3 minutes. The specific steps are: move the heat shield up to 170m above the melting mold, and then move the heat shield down to the original position. The adjustment process is controlled within 3 minutes;

[0077] Turn off the power supply of the graphite electrode, keep the heat shield in the reset and heat preservation position, and keep warm for 3 minutes. Then remove the heat shield and the graphite electrode, end the firing, and obtain the quartz crucible blank.

[0078] Example 5

[0079] This embodiment provides a quartz crucible.

[0080] The difference between this embodiment and embodiment 1 is that the position of the heat shield is not adjusted during the firing process in step S2. The specific steps are as follows:

[0081] Firing: Keep the rotation speed of the melting mold at 70rpm, release the high-temperature arc through the graphite electrode to melt the quartz sand, and keep the inert atmosphere N in the melting furnace during this process. 2 ; The specific details are as follows:

[0082] The melting mold with the crucible blank is kept at a rotation speed of 70 rpm, moved into the arc melting furnace, the graphite electrode is lowered to the middle position of the melting mold, and the heat shield is kept 150m above the melting mold, in the shielding and heat preservation position, and arc melting is started;

[0083] First arc melting: in the time period of 0-30s, the first vacuum degree is controlled to be 0.015Mpa, and the arc current is uniformly increased from zero to the first arc current of 2600A;

[0084] Second arc melting: in the time period of 30-180s, the second vacuum degree is controlled to be 0.095Mpa, and the arc current is uniformly increased from the first arc current of 2600A to the second arc current of 4800A;

[0085] Stable firing: Maintain the second vacuum degree and the second arc starting current unchanged, and perform stable firing for 18 minutes; during the stable firing process, remove the oxide layer every 3 minutes. The specific steps are: move the graphite electrode out of the melting mold, use the blowing device to remove the oxide layer on the graphite electrode, and then move the heat shield and the graphite electrode down to the original position. The process of removing the oxide layer is controlled within 3 minutes;

[0086] Turn off the power supply of the graphite electrode, keep the heat shield in the reset and heat preservation position, and keep warm for 3 minutes. Then remove the heat shield and the graphite electrode, end the firing, and obtain the quartz crucible blank.

[0087] Example 6

[0088] This embodiment provides a quartz crucible.

[0089] The difference between this embodiment and embodiment 1 is that the method for preparing the crucible blank in step S1 is: placing a quartz sand raw material in a melting mold, and performing rotational molding at a rotation speed of 70 rpm to obtain a crucible blank.

[0090] Example 7

[0091] This embodiment provides a quartz crucible.

[0092] The difference between this embodiment and embodiment 1 is that the method for preparing the crucible blank in step S1 is: placing a quartz sand raw material in a melting mold, and performing rotational molding at a rotation speed of 100 pm to obtain a crucible blank.

[0093] Example 8

[0094] This embodiment provides a quartz crucible.

[0095] The difference between this embodiment and embodiment 1 is that: in the method for preparing the crucible blank in step S1: the quartz sand raw materials are different, and the quartz sand raw materials specifically include 10 kg inner layer material, 70 kg middle layer material and 25 kg outer layer material;

[0096] The inner layer material is 80μm quartz sand, 100μm quartz sand and 320μm quartz sand in a weight ratio of 80:33:2; the middle layer material is 80μm quartz sand, 100μm quartz sand and 320μm quartz sand in a weight ratio of 74:19:27; the outer layer material is 80μm quartz sand, 100μm quartz sand and 320μm quartz sand in a weight ratio of 74:13:13.

[0097] Example 9

[0098] This embodiment provides a quartz crucible.

[0099] The difference between this embodiment and embodiment 1 is that: in the method for preparing the crucible blank in step S1: the quartz sand raw materials are different, and the quartz sand raw materials specifically include 10 kg inner layer material, 70 kg middle layer material and 25 kg outer layer material;

[0100] The inner layer material is 80μm quartz sand, 300μm quartz sand and 320μm quartz sand in a weight ratio of 80:33:2; the middle layer material is 80μm quartz sand, 300μm quartz sand and 320μm quartz sand in a weight ratio of 74:19:27; the outer layer material is 80μm quartz sand, 300μm quartz sand and 320μm quartz sand in a weight ratio of 74:13:13.

[0101] Example 10

[0102] This embodiment provides a quartz crucible.

[0103] The difference between this embodiment and embodiment 1 is that: in the method for preparing the crucible blank in step S1: the quartz sand raw materials are different, and the quartz sand raw materials specifically include 10 kg inner layer material, 70 kg middle layer material and 25 kg outer layer material;

[0104] The inner layer material is 80μm quartz sand, 200μm quartz sand and 320μm quartz sand in a weight ratio of 74:19:27; the middle layer material is 80μm quartz sand, 200μm quartz sand and 320μm quartz sand in a weight ratio of 80:33:2; the outer layer material is 80μm quartz sand, 200μm quartz sand and 320μm quartz sand in a weight ratio of 74:13:13.

[0105] Embodiment 11

[0106] This embodiment provides a quartz crucible.

[0107] The difference between this embodiment and embodiment 1 is that: in the method for preparing the crucible blank in step S1: the quartz sand raw materials are different, and the quartz sand raw materials specifically include 10 kg inner layer material, 70 kg middle layer material and 25 kg outer layer material;

[0108] The inner layer material is 80μm quartz sand and 200μm quartz sand in a weight ratio of 74:19; the middle layer material is 80μm quartz sand and 200μm quartz sand in a weight ratio of 80:33; the outer layer material is 80μm quartz sand and 200μm quartz sand in a weight ratio of 74:13.

[0109] Comparative Example

[0110] Comparative Example 1

[0111] This comparative example provides a quartz crucible.

[0112] The preparation method of the quartz crucible in this comparative example is different from that in Example 1 in that the firing process of step S2 is different; specifically, the following steps are included:

[0113] S2: Firing stage: The rotation speed of the melting mold is maintained at 70 rpm, and the high-temperature arc is released through the graphite electrode to melt the quartz sand. During this process, the inert atmosphere N is maintained in the melting furnace. 2 ; The specific details are as follows:

[0114] The melting mold with the crucible blank is kept at a rotation speed of 70 rpm, moved into the arc melting furnace, the graphite electrode is lowered to the middle position of the melting mold, and the heat shield is kept 150m above the melting mold, in the shielding and heat preservation position, and arc melting is started;

[0115] Arc starting and melting: In the time period of 0-30s, the first vacuum degree is controlled to be 0.095Mpa, and the arc starting current is uniformly increased from zero to the first arc starting current of 4800A;

[0116] Stable firing: Maintain the vacuum degree and arc starting current unchanged, and perform stable firing for 18 minutes; during the stable firing process, remove the oxide layer every 3 minutes. The specific steps are: move the heat shield plate up to 170m above the melting mold, and move the graphite electrode out of the melting mold, and use the blowing device to remove the oxide layer on the graphite electrode; then move the heat shield plate and the graphite electrode down to the original position, and the oxide layer removal process is controlled within 3 minutes;

[0117] Turn off the power supply of the graphite electrode, keep the heat shield in the reset and heat preservation position, and keep warm for 3 minutes. Then remove the heat shield and the graphite electrode, end the firing, and obtain the quartz crucible blank.

[0118] Comparative Example 2

[0119] This comparative example provides a quartz crucible.

[0120] The preparation method of the quartz crucible in this comparative example is different from that in Example 1 in that the firing process of step S2 is different; specifically, the following steps are included:

[0121] S2: Firing stage: The rotation speed of the melting mold is maintained at 70 rpm, and the high-temperature arc is released through the graphite electrode to melt the quartz sand. During this process, the inert atmosphere N is maintained in the melting furnace. 2 ; The specific details are as follows:

[0122] The melting mold with the crucible blank is kept at a rotation speed of 70 rpm, moved into the arc melting furnace, the graphite electrode is lowered to the middle position of the melting mold, and the heat shield is kept 150m above the melting mold, in the shielding and heat preservation position, and arc melting is started;

[0123] First arc melting: In the time period of 0-30s, the first vacuum degree is controlled to be 0.03Mpa, and the arc current is uniformly increased from zero to the first arc current of 3400A;

[0124] Second arc melting: in the time period of 30-180s, the second vacuum degree is controlled to be 0.095Mpa, and the arc current is uniformly increased from the first arc current of 2600A to the second arc current of 4800A;

[0125] Stable firing: Maintain the second vacuum degree and the second arc starting current unchanged, and perform stable firing for 18 minutes; during the stable firing process, remove the oxide layer every 3 minutes. The specific steps are: move the heat shield plate up to 170m above the melting mold, and move the graphite electrode out of the melting mold, and use the blowing device to remove the oxide layer on the graphite electrode; then move the heat shield plate and the graphite electrode down to the original position, and the oxide layer removal process is controlled within 3 minutes;

[0126] Turn off the power supply of the graphite electrode, keep the heat shield in the reset and heat preservation position, and keep warm for 3 minutes. Then remove the heat shield and the graphite electrode, end the firing, and obtain the quartz crucible blank.

[0127] Comparative Example 3

[0128] This comparative example provides a quartz crucible.

[0129] The preparation method of the quartz crucible in this comparative example is different from that in Example 1 in that the firing process of step S2 is different; specifically, the following steps are included:

[0130] S2: Firing stage: The rotation speed of the melting mold is maintained at 70 rpm, and the high-temperature arc is released through the graphite electrode to melt the quartz sand. During this process, the inert atmosphere N is maintained in the melting furnace. 2 ; The specific details are as follows:

[0131] The melting mold with the crucible blank is kept at a rotation speed of 70 rpm, moved into the arc melting furnace, the graphite electrode is lowered to the middle position of the melting mold, and the heat shield is kept 150m above the melting mold, in the shielding and heat preservation position, and arc melting is started;

[0132] First arc melting: in the time period of 0-30s, the first vacuum degree is controlled to be 0.015Mpa, and the arc current is uniformly increased from zero to the first arc current of 2600A;

[0133] Second arc melting: in the time period of 30-180s, the second vacuum degree is controlled to be 0.08Mpa, and the arc current is uniformly increased from the first arc current of 2600A to the second arc current of 4000A;

[0134] Stable firing: Maintain the second vacuum degree and the second arc starting current unchanged, and perform stable firing for 18 minutes; during the stable firing process, remove the oxide layer every 3 minutes. The specific steps are: move the heat shield plate up to 170m above the melting mold, and move the graphite electrode out of the melting mold, and use the blowing device to remove the oxide layer on the graphite electrode; then move the heat shield plate and the graphite electrode down to the original position, and the oxide layer removal process is controlled within 3 minutes;

[0135] Turn off the power supply of the graphite electrode, keep the heat shield in the reset and heat preservation position, and keep warm for 3 minutes. Then remove the heat shield and the graphite electrode, end the firing, and obtain the quartz crucible blank.

[0136] Comparative Example 4

[0137] This comparative example provides a quartz crucible.

[0138] The preparation method of the quartz crucible in this comparative example is carried out with reference to the preparation method disclosed in patent CN 115745382 A; the difference from Example 1 is that the firing process of step S2 is different, and specifically includes the following steps:

[0139] S2: Firing stage: In the first stage: time 0-30s, mold speed 76rpm, vacuum 25Hz, current step-by-step increase to 4000A; then the second stage: time 30s-2min45s, mold speed 78rpm, vacuum 50Hz, constant current 3000A; the last stage: time 2min45s-3min, mold speed 81rpm, vacuum 50Hz, constant current 4000A.

[0140] Performance testing

[0141] The quartz crucibles of Examples 1-11 and Comparative Examples 1-4 were used as test objects, and the bulk density, apparent porosity, flexural strength and compressive strength were tested.

[0142] (1) Bulk density and apparent porosity: The test shall be carried out in accordance with GB / T2997-2015 “Test method for bulk density, apparent porosity and true porosity of dense shaped refractory products”.

[0143] (2) Compressive strength: Tested in accordance with GB / T 5072-2008 “Test method for compressive strength of refractory materials at room temperature”.

[0144] Test results: as shown in Table 1.

[0145] Table 1 Performance test results of quartz crucibles in Examples 1-11 and Comparative Examples 1-4

[0146] .

[0147] Combined with Table 1, by comparing the test results of Examples 1-11 with Comparative Examples 1-4, it can be seen that in the process of firing the quartz crucible blank, after the ignition and arcing, within 0-30s, the vacuum degree is set to 0.095Mpa, the arcing current increases from zero to the arcing current of 4800A, and vacuum arcing melting is directly performed, and the performance of the prepared quartz crucible product is poor; when the first vacuum degree is higher than 0.02MPa, or the second vacuum degree is lower than 0.09MPa, the performance of the prepared quartz crucible product is also poor. In the preparation method of the quartz crucible of the present application, the melting mold containing the crucible blank is moved into the arc melting furnace, the graphite electrode is lowered into the melting mold, the arc is started, and at the first vacuum degree, the arc current is increased from zero to the first arc current of 2000-2800A, and vacuum arc melting is performed; at the second vacuum degree, the first arc current is increased to the second arc current of 4600-5000A, and vacuum arc melting is continued; then the second vacuum degree and the second arc current are maintained unchanged, and stable firing is performed for 15-18 minutes, and the arc is cut off and the furnace is taken out to obtain a quartz crucible blank. The above preparation method is used to obtain a volume density higher than 1.72g / cm 3 , a quartz crucible with an apparent porosity lower than 13.9% and a compressive strength higher than 52MPa. The above test results show that the quartz crucible obtained by the preparation method provided by the present application has a lower apparent porosity, a higher volume density, and excellent compressive strength performance of the quartz crucible; and thus a quartz crucible with no bubbles in the inner layer, uniform bubbles in the outer layer, suitable size, and a high yield rate can be obtained.

[0148] By comparing the test results of Examples 1-3, during the process of firing the quartz crucible blank, when the rotation speed of the melting mold is controlled to be 60-80 rpm, the volume density and compressive strength of the quartz crucible can be further improved, and the apparent porosity of the quartz crucible can be reduced.

[0149] By comparing the test results of Examples 1, 4-5, in the process of firing the quartz crucible blank, compared with not removing the oxide layer or not adjusting the position of the heat shield, the present application chooses to adjust the position of the graphite electrode to remove the oxide layer, and adjusts the position of the heat shield, which can further improve the volume density and compressive strength of the quartz crucible and reduce the apparent porosity of the quartz crucible.

[0150] By comparing the test results of Examples 1, 6-7, in the process of preparing the crucible blank in the melting mold, when the rotation speed of the melting mold is controlled to 80-100 rpm, the volume density and compressive strength of the quartz crucible can be further improved, and the apparent porosity of the quartz crucible can be reduced.

[0151] By comparing the test results of Examples 1, 8-11, the present application screens the inner layer material, the middle layer material and the outer layer material in the quartz sand raw material, so that the inner layer material includes 70-100 μm quartz sand, 100-300 μm quartz sand and 300-350 μm quartz sand in a weight ratio of (78-85): (30-45): (1-3), and the middle layer material includes 70-78: (16-22): (24- 30) of 70-100μm quartz sand, 100-300μm quartz sand and 300-350μm quartz sand, and the outer layer material includes 70-100μm quartz sand, 100-300μm quartz sand and 300-350μm quartz sand in a weight ratio of (70-78): (10-16): (10-16), thereby increasing the bulk density and compressive strength of the quartz crucible and reducing the apparent porosity of the quartz crucible.

[0152] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A quartz crucible, characterized in that: The volume density of the quartz crucible is ≥2.08g / cm 3 , apparent porosity ≤10.5%, compressive strength ≥68MPa; The quartz crucible comprises the following components in parts by weight: 8-15 parts of inner layer material, 65-75 parts of middle layer material and 20-28 parts of outer layer material; The inner layer material comprises 70-100 μm quartz sand, 100-300 μm quartz sand and 300-350 μm quartz sand in a weight ratio of (78-85): (30-45): (1-3); The middle layer material comprises 70-100 μm quartz sand, 100-300 μm quartz sand and 300-350 μm quartz sand in a weight ratio of (70-78): (16-22): (24-30); The outer layer material comprises 70-100 μm quartz sand, 100-300 μm quartz sand and 300-350 μm quartz sand in a weight ratio of (70-78): (10-16): (10-16); The preparation method of the quartz crucible is as follows: the quartz crucible is obtained by a firing process, and the firing process includes the following steps: The quartz sand raw material is subjected to rotational molding at a rotation speed of 85-95 rpm to obtain a quartz crucible blank; Under the conditions of inert atmosphere and rotation speed of 65-75rpm, the quartz crucible blank is continuously subjected to the following steps: First arc melting: In the time period of 0-(25-35)s, the first vacuum degree is controlled to be 0.01-0.02Mpa, and the arc current is uniformly increased from zero to the first arc current of 2000-2800A; Second arc melting: in the time period of (25-35)-(150-210) s, the second vacuum degree is controlled to be 0.09-0.1Mpa, and the arc current is uniformly increased from the first arc current to the second arc current of 4600-5000A; Stable firing: maintaining the second vacuum degree and the second arc starting current unchanged, and performing stable firing for 15-18 minutes; The firing process is implemented using an arc melting furnace, which includes a melting mold, a graphite electrode, a heat shield, an air blowing device, a compressed air nozzle, and an exhaust pipe; During the stable firing process, the oxide layer is removed every 2-3 minutes, and the specific steps are: the graphite electrode is moved out of the melting mold, the oxide layer on the graphite electrode is removed by the blowing device, and then the graphite electrode is moved down to the original position in the melting mold, and then the stable firing is performed; the oxide layer removal process is controlled within 3 minutes; Before the first arc melting, the heat shield is arranged to be located 130-150m above the melting mold; during the stable firing process, in the process of removing the oxide layer every 2-3 minutes, the position of the heat shield needs to be adjusted, and the specific steps are: moving the heat shield upward to 160-180m above the melting mold, and then moving the graphite electrode out of the melting mold. After the oxide layer removal operation is completed, the heat shield and the graphite electrode are moved down to the original position, and then the stable firing is carried out; the adjustment process is controlled within 3 minutes.

2. The quartz crucible according to claim 1, characterized in that: The size of the quartz crucible is 32-36 inches.

3. The method for preparing a quartz crucible according to any one of claims 1 to 2, characterized in that: The quartz crucible is obtained by a firing process, and the firing process comprises the following steps: Under the conditions of inert atmosphere and rotation speed of 60-80rpm, the quartz crucible blank is continuously subjected to the following steps: First arc melting: In the time period of 0-(25-35)s, the first vacuum degree is controlled to be 0.01-0.02Mpa, and the arc current is uniformly increased from zero to the first arc current of 2000-2800A; Second arc melting: in the time period of (25-35)-(150-210) s, the second vacuum degree is controlled to be 0.09-0.1Mpa, and the arc current is uniformly increased from the first arc current to the second arc current of 4600-5000A; Stable firing: the second vacuum degree and the second arc starting current are maintained unchanged, and stable firing is performed for 15-18 minutes.