A preparation process of silver-spotted Tianmu raindrop glaze porcelain
By optimizing the ratio of carcass and glaze, combined with specific firing processes and temperature control, the problem of instability of raindrop glaze during the production process is solved, the reliability and economic benefits of the finished product are improved, and the glaze oiling is achieved Stable improvement in drip effect.
Patent Information
- Application Number
- CN202310366451.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-04-03
AI Technical Summary
Raindrop glaze has strong instability during the production process. The temperature level determines its success or failure. The temperature difference cannot exceed 5 degrees, and it is difficult to fire, resulting in accidental and uncertainty in the finished product effect.
The optimized carcass and glaze ratio composition is: zircon is added to the carcass, and the glaze contains zircon, montmorillonite, boronite and other components, and the glaze slurry is prepared through specific mixing and grinding processes. Combined with natural drying and kiln firing processes, the firing temperature is controlled at 1180-1270 degrees, and a variety of glaze methods and redox atmospheres are used to perform high-temperature glaze firing.
The yield rate of oil droplets on the glaze surface is significantly improved, production costs are reduced, and the reliability and economic benefits of raindrop molding effect are improved, and the problems of accidental and uncertainty of finished products in the prior art are solved.
Abstract
Description
Technical Field
[0001] The invention relates to the field of pottery preparation technology, in particular to a preparation technology of silver-spotted Tianmu raindrop glaze porcelain. Background Art
[0002] Raindrop glaze ceramics were famous for tea-fighting in ancient times and are treasures for collectors today. Raindrop glaze is called "China's wonder and ceramic mystery" by domestic and foreign guests for its calm, elegant, dignified and noble artistic style. Raindrop glaze is called "Tenmoku glaze" in Japan and is a fine tea set for Japanese tea ceremony. If you pour tea into it, the spots will shine like Venus, and if you pour water or white wine into it, the silver stars will sparkle and glitter, giving people a sense of beauty. When people contemplate and observe the works of raindrop glaze, they will add a wonderful artistic conception of "a dark night with no clouds and full of stars". The best raindrop glaze is deep, the glaze bottom is black and shiny, the glaze surface is flat, the silver star points are full and symmetrical, the crystals are round and shiny, and the crystal points are as big as beans and as small as millet, which resembles the water circle spots of raindrops falling into the water.
[0003] However, raindrop glaze is very unstable during the production process. The success or failure of "raindrop glaze" is determined by the temperature. The temperature difference cannot exceed 5 degrees. If it is too high, the crystals will be burned out, and if it is too low, no crystals will appear, making firing more difficult. Summary of the invention
[0004] According to the above technical problems, the present invention provides a preparation process of silver-spotted Tianmu raindrop glaze porcelain, wherein the Tianmu raindrop glaze comprises a body and a glaze.
[0005] The raw material composition of the matrix is: quartz 40-50 parts, pyroxene 5-10 parts, orthoclase 3-5 parts, zircon 6-12 parts, bauxite 3-6 parts, white kaolin 10-15 parts, bentonite 10-15 parts, clay 5-10 parts, and binder 1-5 parts;
[0006] The optimal ratio of the matrix raw materials is: 42 parts of quartz, 6 parts of pyroxene, 3 parts of orthoclase, 7 parts of zircon, 3 parts of bauxite, 12 parts of white kaolin, 11 parts of bentonite, 7 parts of clay and 3 parts of binder.
[0007] The raw material composition of the glaze is: 25-35 parts of zircon, 15-18 parts of montmorillonite, 12-15 parts of magnesite, 8-12 parts of talc, 6 parts of potassium feldspar, 6 parts of barium carbonate, 2 parts of copper, 3-5 parts of zinc oxide, 0.3-0.5 parts of manganese oxide, 1-2 parts of tin oxide, 0.5-1 parts of titanium oxide, 1.5-2.5 parts of iron oxide, and 3-5 parts of matte frit;
[0008] The optimal proportion of the glaze is: 30 parts of zircon, 17 parts of montmorillonite, 12 parts of magnesite, 9 parts of talc, 6 parts of potassium feldspar, 6 parts of barium carbonate, 2 parts of copper, 3 parts of zinc oxide, 0.3 parts of manganese oxide, 1 part of tin oxide, 0.6 parts of titanium oxide, 1.5 parts of iron oxide, and 4 parts of matte frit.
[0009] The preparation process comprises the following steps:
[0010] Step 1: Mix the carcass raw materials in the best ratio and add them to the grinder, add water in a ratio of 1:1 for wet grinding, pass through a 260-mesh sieve to obtain glaze slurry, and then form the required blank by slip injection, embryo pulling or other mechanical forming methods;
[0011] Step 2: After the blank is made, it is dried in a natural state for more than 24 hours, and then put into a kiln for biscuit firing at 700-1000 degrees for 5-6 hours. After the blank is sintered, its water absorption rate is less than 1%, and then it is cooled to room temperature. Biscuit firing is used to improve the strength of the blank;
[0012] Step 3, crushing and mixing the glaze materials according to the optimal ratio, and grinding them by a ball mill to obtain a glaze slurry;
[0013] Step 4: Use glaze slurry to glaze the blank. There are many glazing methods, such as dipping glaze, swinging glaze, pouring glaze, brushing glaze, blowing glaze, wheel glaze, etc.
[0014] Step 5: After the glaze slurry used to glaze the blank is dried, it is sent into a kiln for high-temperature glaze firing at a temperature ranging from 1180 to 1270 degrees Celsius in an oxidation-reduction atmosphere.
[0015] The firing temperature is specifically controlled as follows:
[0016] Low temperature stage: from room temperature to 600-700 degrees, the firing time is 1-3 hours;
[0017] Medium temperature stage: the temperature rises to 850-1000 degrees, and the firing time is 2-4 hours;
[0018] High temperature stage: the temperature in the kiln rises to 1180-1270 degrees, and the firing time is 3-4 hours;
[0019] Insulation stage: control the temperature in the furnace within the range of 1230-1270, and the firing time is 2-3 hours;
[0020] Cooling stage: Cool down the furnace to room temperature and cool naturally.
[0021] Beneficial effects of the present invention:
[0022] The invention introduces zircon into both the body raw material and the glaze raw material, which can greatly improve the body and the glaze through high-temperature integrated firing and reduce the cost of production input.
[0023] The firing method of the present invention can significantly improve the yield rate of the oil drop effect on the glaze surface and obtain outstanding economic benefits. After adopting the glaze formula and firing method of the present invention, the number of porcelains with good raindrop forming effect can be increased after each firing. Compared with the randomness and uncertainty of obtaining the raindrop effect in the prior art, the present invention has obvious technical progress. DETAILED DESCRIPTION
[0024] The present invention is further described in detail in conjunction with the following specific examples, and the protection scope of the present invention is not limited to the following examples. The process, conditions, reagents, experimental methods, etc. for implementing the present invention, except for the contents specifically mentioned below, are all common knowledge and common common sense in the art, and the present invention has no special restrictions.
[0025] A preparation process of silver-spotted Tianmu raindrop glaze porcelain, wherein the Tianmu raindrop glaze comprises a body and a glaze, wherein the raw materials of the body are composed of: 40-50 parts of quartz, 5-10 parts of pyrope, 3-5 parts of orthoclase, 6-12 parts of zircon, 3-6 parts of bauxite, 10-15 parts of white kaolin, 10-15 parts of bentonite, 5-10 parts of clay, and 1-5 parts of a binder;
[0026] The optimal ratio of the matrix raw materials is: 42 parts of quartz, 6 parts of pyroxene, 3 parts of orthoclase, 7 parts of zircon, 3 parts of bauxite, 12 parts of white kaolin, 11 parts of bentonite, 7 parts of clay and 3 parts of binder.
[0027] The raw material composition of the glaze is: 25-35 parts of zircon, 15-18 parts of montmorillonite, 12-15 parts of magnesite, 8-12 parts of talc, 6 parts of potassium feldspar, 6 parts of barium carbonate, 2 parts of copper, 3-5 parts of zinc oxide, 0.3-0.5 parts of manganese oxide, 1-2 parts of tin oxide, 0.5-1 parts of titanium oxide, 1.5-2.5 parts of iron oxide, and 3-5 parts of matte frit;
[0028] The optimal proportion of the glaze is: 30 parts of zircon, 17 parts of montmorillonite, 12 parts of magnesite, 9 parts of talc, 6 parts of potassium feldspar, 6 parts of barium carbonate, 2 parts of copper, 3 parts of zinc oxide, 0.3 parts of manganese oxide, 1 part of tin oxide, 0.6 parts of titanium oxide, 1.5 parts of iron oxide, and 4 parts of matte frit.
[0029] The preparation process comprises the following steps:
[0030] Step 1: Mix the carcass raw materials in the best ratio and add them to the grinder, add water in a ratio of 1:1 for wet grinding, pass through a 260-mesh sieve to obtain glaze slurry, and then form the required blank by slip injection, embryo pulling or other mechanical forming methods;
[0031] Step 2: After the blank is made, it is dried in a natural state for more than 24 hours, and then put into a kiln for biscuit firing at 700-1000 degrees for 5-6 hours. After the blank is sintered, its water absorption rate is less than 1%, and then it is cooled to room temperature. Biscuit firing is used to improve the strength of the blank;
[0032] Step 3, crushing and mixing the glaze materials according to the optimal ratio, and grinding them by a ball mill to obtain a glaze slurry;
[0033] Step 4: Use glaze slurry to glaze the blank. There are many glazing methods, such as dipping glaze, swinging glaze, pouring glaze, brushing glaze, blowing glaze, wheel glaze, etc.
[0034] Step 5: After the glaze slurry used to glaze the blank is dried, it is sent into a kiln for high-temperature glaze firing at a temperature ranging from 1180 to 1270 degrees Celsius in an oxidation-reduction atmosphere.
[0035] The firing temperature is specifically controlled as follows:
[0036] Low temperature stage: from room temperature to 600-700 degrees, the firing time is 1-3 hours;
[0037] Medium temperature stage: the temperature rises to 850-1000 degrees, and the firing time is 2-4 hours;
[0038] High temperature stage: the temperature in the kiln rises to 1180-1270 degrees, and the firing time is 3-4 hours;
[0039] Insulation stage: control the temperature in the furnace within the range of 1230-1270, and the firing time is 2-3 hours;
[0040] Cooling stage: Cool down the furnace to room temperature and cool naturally.
[0041] Example 1
[0042] A spotted Tianmu raindrop glaze porcelain comprises a body and a glaze, wherein the body is composed of the following weight ratio: 45 parts of quartz, 6 parts of charcoal gemstone, 4 parts of orthoclase, 8 parts of zircon, 3 parts of bauxite, 15 parts of white kaolin, 10 parts of bentonite, 7 parts of clay and 3 parts of a binder.
[0043] The glaze is composed of the following weight ratio: 25 parts of zircon, 15 parts of montmorillonite, 15 parts of magnesite, 8 parts of talc, 6 parts of potassium feldspar, 6 parts of barium carbonate, 2 parts of copper, 5 parts of zinc oxide, 0.4 parts of manganese oxide, 1 part of tin oxide, 0.5 parts of titanium oxide, 1.8 parts of iron oxide, and 5 parts of matte frit.
[0044] The preparation process steps are as follows:
[0045] Step 1: Mix the carcass raw materials in proportion and add them into a grinder, grind them with water in a ratio of 1:1, pass through a 260-mesh sieve to obtain glaze slurry, and then plasticize them into blanks by slip injection;
[0046] Step 2: After the blank is made, it is dried in a natural state for more than 24 hours, and then put into the kiln for biscuit firing at 700 degrees for 5 hours. After the blank is sintered, its water absorption rate is less than 1%, and then it is cooled to room temperature. Biscuit firing is used to improve the strength of the blank;
[0047] Step 3, crushing and mixing the glaze materials according to the optimal ratio, and grinding them by a ball mill to obtain a glaze slurry;
[0048] Step 4, glazing the blank once or more than once by dipping the glaze slurry;
[0049] Step 5: After the glaze slurry applied to the blank is dried, it is sent into the kiln for high-temperature glaze firing in the range of 1230°C under an oxidation-reduction atmosphere. The firing temperature is specifically controlled as follows:
[0050] Low temperature stage: from room temperature to 600 degrees, the firing time is 2 hours;
[0051] Medium temperature stage: the temperature is raised to 850 degrees and the firing time is 2 hours;
[0052] High temperature stage: the temperature in the kiln rises to 1180 degrees and the firing time is 3 hours;
[0053] Insulation stage: control the temperature in the furnace within the range of 1230°C and the firing time is 2 hours;
[0054] Cooling stage: The temperature in the furnace is cooled down to room temperature, and the finished product is obtained after natural cooling.
[0055] Example 2
[0056] A spotted Tianmu raindrop glaze porcelain comprises a body and a glaze, wherein the body is composed of the following weight ratio: 43 parts of quartz, 6 parts of charcoal gemstone, 5 parts of orthoclase, 6 parts of zircon, 4 parts of bauxite, 13 parts of white kaolin, 10 parts of bentonite, 6 parts of clay and 2 parts of a binder.
[0057] The glaze is composed of the following weight ratio: 35 parts of zircon, 18 parts of montmorillonite, 14 parts of magnesite, 10 parts of talc, 6 parts of potassium feldspar, 6 parts of barium carbonate, 2 parts of copper, 4 parts of zinc oxide, 0.3 parts of manganese oxide, 1 part of tin oxide, 0.7 parts of titanium oxide, 1.6 parts of iron oxide, and 3 parts of matte frit.
[0058] The preparation process steps are as follows:
[0059] Step 1: Mix the carcass raw materials in proportion and add them into a grinder, grind them with water in a ratio of 1:1, pass through a 260-mesh sieve to obtain glaze slurry, and then plasticize them into blanks by slip injection;
[0060] Step 2: After the blank is made, it is dried in a natural state for more than 24 hours, and then put into the kiln for biscuit firing at 750 degrees for 5 hours. After the blank is sintered, its water absorption rate is less than 1%, and then it is cooled to room temperature. Biscuit firing is used to improve the strength of the blank;
[0061] Step 3, crushing and mixing the glaze materials according to the optimal ratio, and grinding them by a ball mill to obtain a glaze slurry;
[0062] Step 4, glazing the blank once or more than once by dipping the glaze slurry;
[0063] Step 5: After the glaze slurry applied to the blank is dried, it is sent into the kiln for high-temperature glaze firing in an oxidation-reduction atmosphere at a temperature within the range of 1250°C. The firing temperature is specifically controlled as follows:
[0064] Low temperature stage: from room temperature to 700 degrees, the firing time is 1.5 hours;
[0065] Medium temperature stage: the temperature is raised to 850 degrees and the firing time is 3 hours;
[0066] High temperature stage: the temperature in the kiln rises to 1230 degrees and the firing time is 3.5 hours;
[0067] Insulation stage: control the temperature in the furnace within the range of 1250°C and the firing time is 2 hours;
[0068] Cooling stage: The temperature in the furnace is cooled down to room temperature, and the finished product is obtained after natural cooling.
[0069] Example 3
[0070] A spotted Tianmu raindrop glaze porcelain comprises a body and a glaze, wherein the body is composed of the following weight ratio: 42 parts of quartz, 6 parts of charcoal gemstone, 3 parts of orthoclase, 7 parts of zircon, 3 parts of bauxite, 12 parts of white kaolin, 11 parts of bentonite, 7 parts of clay and 3 parts of a binder.
[0071] The glaze is composed of the following weight ratio: 30 parts of zircon, 17 parts of montmorillonite, 12 parts of magnesite, 9 parts of talc, 6 parts of potassium feldspar, 6 parts of barium carbonate, 2 parts of copper, 3 parts of zinc oxide, 0.3 parts of manganese oxide, 1 part of tin oxide, 0.6 parts of titanium oxide, 1.5 parts of iron oxide, and 4 parts of matte frit.
[0072] The preparation process steps are as follows:
[0073] Step 1: Mix the carcass raw materials in proportion and add them into a grinder, grind them with water in a ratio of 1:1, pass through a 260-mesh sieve to obtain glaze slurry, and then plasticize them into blanks by slip injection;
[0074] Step 2: After the blank is made, it is dried in a natural state for more than 24 hours, and then put into the kiln for biscuit firing at 750 degrees for 5.5 hours. After the blank is sintered, its water absorption rate is less than 1%, and then it is cooled to room temperature. Biscuit firing is used to improve the strength of the blank;
[0075] Step 3, crushing and mixing the glaze materials according to the optimal ratio, and grinding them by a ball mill to obtain a glaze slurry;
[0076] Step 4, glazing the blank once or more than once by dipping the glaze slurry;
[0077] Step 5: After the glaze slurry applied to the blank is dried, it is sent into the kiln for high-temperature glaze firing in an oxidation-reduction atmosphere at a temperature within the range of 1250°C. The firing temperature is specifically controlled as follows:
[0078] Low temperature stage: from room temperature to 700 degrees, the firing time is 2 hours;
[0079] Medium temperature stage: the temperature is raised to 800 degrees and the firing time is 2.5 hours;
[0080] High temperature stage: the temperature in the kiln rises to 1230 degrees and the firing time is 3 hours;
[0081] Insulation stage: control the temperature in the furnace within the range of 1250°C and the firing time is 2 hours;
[0082] Cooling stage: The temperature in the furnace is cooled down to room temperature, and the finished product is obtained after natural cooling.
[0083] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. The various components mentioned in the present invention are common technologies in the existing field. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only to illustrate the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.
Claims
1. A preparation process of silver-spotted Tianmu raindrop glaze porcelain, wherein the Tianmu raindrop glaze comprises a body and a glaze, wherein the weight ratio of the body raw materials is: 40-50 parts of quartz, 5-10 parts of pyrope, 3-5 parts of orthoclase, 6-12 parts of zircon, 3-6 parts of bauxite, 10-15 parts of white kaolin, 10-15 parts of bentonite, 5-10 parts of clay, and 1-5 parts of a binder, and the weight ratio of the glaze raw materials is: The composition ratio is: 25-35 parts of zircon, 15-18 parts of montmorillonite, 12-15 parts of magnesite, 8-12 parts of talc, 6 parts of potassium feldspar, 6 parts of barium carbonate, 2 parts of copper, 3-5 parts of zinc oxide, 0.3-0.5 parts of manganese oxide, 1-2 parts of tin oxide, 0.5-1 parts of titanium oxide, 1.5-2.5 parts of iron oxide, 3-5 parts of matte frit, high temperature glaze firing in an oxidation-reduction atmosphere, the firing temperature is controlled The system is as follows: Low temperature stage: from room temperature to 600-700 degrees, the firing time is 1-3 hours; Medium temperature stage: the temperature rises to 850-1000 degrees, and the firing time is 2-4 hours; High temperature stage: the temperature in the kiln rises to 1180-1270 degrees, and the firing time is 3-4 hours; Insulation stage: control the temperature in the furnace within the range of 1230-1270 degrees, and the firing time is 2-3 hours; Cooling stage: Cool down the furnace to room temperature and cool naturally.
2. The preparation process of the silver-spotted Tianmu raindrop glaze porcelain according to claim 1, characterized in that The weight ratio of the matrix raw materials is as follows: 42 parts of quartz, 6 parts of pyroxene, 3 parts of orthoclase, 7 parts of zircon, 3 parts of bauxite, 12 parts of white kaolin, 11 parts of bentonite, 7 parts of clay and 3 parts of binder.
3. The preparation process of the silver-spotted Tianmu raindrop glaze porcelain according to claim 1 is characterized in that The following steps are involved: Step 1: Mix the carcass raw materials in a certain proportion and add them into a grinder. Add water in a ratio of 1:1 for wet grinding. After grinding, pass through a 260-mesh sieve to obtain glaze slurry, and then form the desired blank by slip injection, embryo pulling or other mechanical forming methods. Step 2: After the blank is made, it is dried in a natural state for more than 24 hours, and then put into a kiln for biscuit firing at 700-1000 degrees for 5-6 hours. After the blank is sintered, its water absorption rate is less than 1%, and then it is cooled to room temperature. Biscuit firing is used to improve the strength of the blank; Step 3, crushing and mixing the glaze materials according to the proportion, and grinding them by a ball mill to obtain a glaze slurry; Step 4: glaze the blank with glaze slurry. The glazing methods include dipping glaze, swinging glaze, pouring glaze, brushing glaze, blowing glaze and wheel glaze; Step 5: After the glaze slurry used to glaze the blank is dry, it is sent into the kiln for high-temperature glaze firing.