A high entropy alloy based on rare earth alloying and its composition design method
Through the alloying of rare earth elements Gd or La, the dendrite phase and the interdendrite phase are formed, which solves the problem of insufficient strength of CoCrFeNi high-entropy alloy, improves its application potential in the field of structural materials, and optimizes the component design efficiency.
Patent Information
- Application Number
- CN202310710092.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-06-15
AI Technical Summary
CoCrFeNi high-entropy alloys have excellent plasticity but low strength in the field of structural materials, resulting in limited promotion, and the design efficiency and large workload of existing rare earth alloys.
The rare earth elements Gd or La are used for alloying. By selecting rare earth elements with a large difference in atomic radius from CoCrFeNi high-entropy alloy, the dendrite phase and the interdrite phase are formed, the microstructure structure of the alloy is optimized, and the strength and plasticity are improved.
It achieves the significant improvement of the strength of high-entropy alloy while maintaining good plasticity, forming a variety of strong plasticity combinations, and optimizing the overall performance of the alloy.
Smart Images

Figure CN116732414B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of high entropy alloys, in particular to a high entropy alloy based on rare earth alloying and a composition design method thereof. Background Art
[0002] High entropy alloy was formally proposed by Ye Junwei at the beginning of this century. Due to its own unique four effects, high entropy alloy has a series of excellent properties such as thermal stability, high strength and toughness, fatigue resistance, corrosion resistance, etc. At the same time, high entropy alloy can form a single-phase solid solution with different performance characteristics such as FCC, BCC and HCP in terms of organization. In recent years, high entropy alloy has attracted much attention in the field of structural materials and functional materials, and is expected to serve in the fields of aerospace and manufacturing.
[0003] CoCrFeNi high entropy alloy has a single-phase FCC structure, so CoCrFeNi high entropy alloy has been widely promoted in the field of structural materials due to its excellent plasticity of the FCC phase. However, its strength is average in practical engineering applications. In the field of traditional alloys, rare earth element alloying is an effective method to optimize the mechanical properties of alloys. However, the effects of different rare earth elements on the properties of CoCrFeNi high entropy alloys at different addition amounts vary greatly. Directly studying the effects of rare earth element alloying on the plasticity and mechanical strength of CoCrFeNi high entropy alloys through experiments has the disadvantages of low efficiency and large workload. Summary of the invention
[0004] To this end, the technical problem to be solved by the present invention is to provide a high-entropy alloy based on rare earth alloying and a composition design method thereof, so as to solve the problem that the existing CoCrFeNi high-entropy alloy has excellent plasticity but low strength, which leads to its limited promotion in the field of structural materials, and the problem that the existing rare earth alloying high-entropy alloy composition design method is low in efficiency and has a large workload.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A rare earth alloy-based high entropy alloy with the chemical formula (CoCrFeNi) 100-x RE x RE is a rare earth element, and the value of X is 0.05-3at.%. The present invention is based on the design concept of rare earth alloying, and applies the method of optimizing alloy microstructure and performance by rare earth alloying, which is widely used in traditional alloys, to high entropy alloys; a single-phase FCC structured CoCrFeNi high entropy alloy is selected as a matrix alloy, and rare earth elements Gd and La are selected as additive elements; the single-phase FCC high entropy alloy CoCrFeNi has excellent plasticity but average strength performance, and after rare earth alloying, the strengthening effect of forming a new phase due to the addition of rare earth is highlighted.
[0007] In the above rare earth alloy-based high entropy alloy, RE is a rare earth element gadolinium Gd or lanthanum La; and the value of X is 0.05 at.%, 0.1 at.%, 0.3 at.%, 0.5 at.%, 1.0 at.%, 2.0 at.% or 3.0 at.%.
[0008] The rare earth alloy-based high entropy alloy has a dendrite phase and an interdendritic phase; the dendrite phase is an FCC phase, and the interdendritic phase is a hexagonal structure HS phase.
[0009] A composition design method based on rare earth alloying high entropy alloy comprises the following steps:
[0010] Step (1), according to the lattice distortion effect, select a rare earth element with a large difference in atomic radius from the four main elements of the CoCrFeNi high entropy alloy as an additive element to prepare a high entropy alloy having a chemical formula of (CoCrFeNi): 100-x RE x Rare earth alloyed high entropy alloy, RE is a rare earth element;
[0011] Step (2), determine (CoCrFeNi) 100-x RE x The contents of the four main elements in the rare earth alloy high entropy alloy make it meet the standards of the second generation high entropy alloy;
[0012] Step (3), determine the amount of the added element in the CoCrFeNi high entropy alloy so that the designed (CoCrFeNi) 100-x RE x The atomic percentage X value of the medium rare earth element RE is 0.05 to 3.0 at.%; if the rare earth element addition amount is less than 0.05 at.%, only a small amount of rare earth enriched area can be formed but no second phase can be formed; if the rare earth element addition amount is higher than 3.0 at.%, in addition to the rare earth phase, a large amount of rare earth enriched area will be generated, resulting in deterioration of alloy performance;
[0013] Step (4), according to the designed (CoCrFeNi) 100-x RE x Preparation of rare earth alloyed high entropy alloys with different added elements and rare earth alloyed high entropy alloys with different added elements;
[0014] Step (5), preparing the rare earth alloy high entropy alloy (CoCrFeNi) in step (4) 100-x RE x The microstructure and mechanical properties were compared, and rare earth alloyed high entropy alloys with excellent comprehensive properties of strong plasticity and strong strength were screened out.
[0015] In the above-mentioned composition design method based on rare earth alloying high entropy alloy, in step (1), rare earth elements whose atomic radius difference with the component elements in CoCrFeNi high entropy alloy is between 40 and 60 pm are defined as rare earth elements with large atomic radius difference.
[0016] In the composition design method based on rare earth alloying high entropy alloy, in step (1), rare earth element gadolinium Gd or lanthanum La is selected as the added element; compared with other rare earth elements that meet the atomic radius difference, the rare earth high entropy alloy prepared by adding light rare earth La or medium rare earth Gd has more stable and excellent performance.
[0017] The CoCrFeNi high entropy alloy has a FCC single-phase structure. The atomic radius of the main element Co is 135±5pm, the atomic radius of Cr is 140±5pm, the atomic radius of Fe is 140±5pm, and the atomic radius of Ni is 135±5pm. The difference between the atomic radii of the four main elements is very small. According to the lattice distortion effect among the four core effects of high entropy alloys, the degree of lattice distortion of the CoCrFeNi high entropy alloy microstructure when forming an FCC single-phase solid solution is relatively small; the atomic radius of the rare earth element Gd is 180±5pm, and the atomic radius of the rare earth element La is 195±5pm. The difference between the two and the atomic radius of the four main elements of the matrix alloy CoCrFeNi is 40pm and 55pm respectively, which is a large difference. When Gd or La is added to form a solid solution, it will cause a large lattice distortion, and the internal distortion energy is large. Based on the lattice distortion effect, one of the core effects of high entropy alloys, the atomic radius of rare earth elements La and Gd is quite different from the atomic radius of the four main elements of CoCrFeNi high entropy alloys, which further promotes the effect of strengthening the alloy by increasing the internal distortion energy of the alloy system due to the lattice distortion effect.
[0018] In the above-mentioned composition design method based on rare earth alloying high entropy alloy, in step (2), the contents of the four main elements of the CoCrFeNi high entropy alloy are determined as follows: the atomic percentage of cobalt Co is 5 to 35 at.%, the atomic percentage of chromium Cr is 5 to 35 at.%, the atomic percentage of iron Fe is 5 to 35 at.%, and the atomic percentage of nickel Ni is 5 to 35 at.%.
[0019] In the above-mentioned composition design method based on rare earth alloying high entropy alloy, the atomic percentage ratio of the four main elements in the CoCrFeNi high entropy alloy is 1:1:1:1.
[0020] In the above-mentioned composition design method based on rare earth alloying high entropy alloy, in step (3), the value of X is 0.05at.%, 0.1at.%, 0.3at.%, 0.5at.%, 1.0at.%, 2.0at.% or 3.0at.%, wherein 0.05-0.5at.% is a very trace addition, and 1.0-3.0at.% is a trace addition; from the gradient change of the addition amount, it is more perfect (CoCrFeNi) 100- x RE x Alloy system.
[0021] In the above-mentioned composition design method based on rare earth alloying high entropy alloy, in step (4), the rare earth alloying high entropy alloy (CoCrFeNi) 100-x RE x Prepared by vacuum arc melting:
[0022] Step (4-1), according to the rare earth alloy high entropy alloy (CoCrFeNi) 100-x RE x The alloy raw materials are prepared according to the proportion of each element in the raw materials; the purity of the raw materials used is greater than or equal to 99.99wt%;
[0023] Step (4-2), placing the alloy raw material in a vacuum arc melting device for melting to obtain alloy raw material liquid;
[0024] Step (4-3), casting the alloy raw material liquid, and naturally cooling to room temperature after casting, to obtain a rare earth alloy high entropy alloy (CoCrFeNi) 100-x RE x .
[0025] The present invention is based on (CoCrFeNi) 100-x RE x The cast alloy prepared by (RE=Gd, La, X=0.05, 0.1, 0.3, 0.5, 1.0, 2.0, 3.0at.%), in terms of microstructure, firstly, a new phase is formed, and the formation of the new phase has a direct contribution to the strength of the alloy. Secondly, the grains of the alloy structure after adding rare earth Gd and La are significantly refined; in terms of mechanical properties, the plasticity of the alloy with different Gd and La addition amounts in the whole system decreases slightly to varying degrees, but the strength is significantly improved. After adding rare earth Gd and La, the alloy structure is distributed in a dendritic state, and the alloy phase changes from FCC single phase to dendritic phase (DR) and interdendritic phase (ID), among which the dendritic phase (DR) is FCC phase, and the interdendritic phase (ID) is hexagonal structure phase (HS phase); different rare earth elements are used as additive elements to prepare (CoCrFeNi) 100-x RE xCompared with the CoCrFeNi high-entropy alloy, the alloy has a different degree of grain refinement and a different amount of interdendritic HS phase, thus forming a variety of strength-plasticity combinations, which can be compared to obtain the optimal one, that is, the alloy with the best comprehensive strength-plasticity performance in the new alloy system.
[0026] The technical solution of the present invention achieves the following beneficial technical effects:
[0027] A novel high entropy alloy (CoCrFeNi) of rare earth element alloying system is designed by the composition design method of the present invention. 100-x RE x (RE = Gd, La, X = 0.05, 0.1, 0.3, 0.5, 1, 2, 3 at.%); Utilize the influence of rare earth elements with specific atomic radius on the microstructure of the alloy, so as to improve the strength of the matrix high entropy alloy while maintaining good plasticity. Based on rare earth alloying (CoCrFeNi) 100-x RE x The (RE = Gd, La, X = 0.05, 0.1, 0.3, 0.5, 1, 2, 3 at.%) series alloys show relatively large benign changes in microstructure, especially in the refinement of grain size. In terms of alloy phase, rare earth addition forms a new phase that significantly contributes to the strength of the alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1a The microstructure of the CoCrFeNi alloy in Example 1 of the present invention;
[0029] Figure 1b In Example 1 of the present invention (CoCrFeNi) 99 Microstructure of Gd1 alloy;
[0030] Figure 1c In Example 1 of the present invention (CoCrFeNi) 97 Microstructure of Gd3 alloy;
[0031] Figure 2 In Example 1 of the present invention, the CoCrFeNi alloy (CoCrFeNi) 99 Gd1 alloy and (CoCrFeNi) 97 Compressive stress-strain curve of Gd3 alloy;
[0032] Figure 3a The microstructure of the CoCrFeNi alloy in Example 2 of the present invention;
[0033] Figure 3b In Example 2 of the present invention (CoCrFeNi) 99 Microstructure of La1 alloy;
[0034] Figure 3c In Example 2 of the present invention (CoCrFeNi) 98 Microstructure of La2 alloy;
[0035] Figure 4 In Example 2 of the present invention, the CoCrFeNi alloy (CoCrFeNi) 99 La1 alloy and (CoCrFeNi) 98 Compressive stress-strain curve of La2 alloy. DETAILED DESCRIPTION
[0036] Example 1
[0037] This embodiment is based on the composition design method of rare earth alloyed high entropy alloy, comprising the following steps:
[0038] Step (1), according to the lattice distortion effect, select a rare earth element with a large difference in atomic radius from the four main elements of the CoCrFeNi high entropy alloy as an additive element to prepare a high entropy alloy having a chemical formula of (CoCrFeNi): 100-x RE x Rare earth alloyed high entropy alloy, RE is a rare earth element;
[0039] Step (2), determine (CoCrFeNi) 100-x G x The contents of the four main elements in the rare earth alloy high entropy alloy meet the standards of the second generation high entropy alloy. In this embodiment, the atomic percentage ratio of the four main elements in the CoCrFeNi high entropy alloy is 1:1:1:1; the rare earth element is gadolinium Gd;
[0040] Step (3), determine the amount of the added element in the CoCrFeNi high entropy alloy so that the designed (CoCrFeNi) 100-x G x The atomic percentage X value of the medium rare earth element Gd is 0.05 to 3.0 at.%;
[0041] Step (4), according to the designed (CoCrFeNi) 100-x G x Preparation of rare earth alloyed high entropy alloys with different added elements and rare earth alloyed high entropy alloys with different added elements; rare earth alloyed high entropy alloy (CoCrFeNi) 100-x G x The preparation method is:
[0042] Step (4-1), according to the rare earth alloy high entropy alloy (CoCrFeNi) 100-x G xThe alloy raw materials are prepared according to the proportion of each element in the alloy raw materials; the purity of the alloy raw materials used is greater than or equal to 99.99wt%;
[0043] Step (4-2), placing all alloy raw materials into a vacuum arc melting device for melting at the same time to obtain alloy raw material liquid;
[0044] Step (4-3), casting the alloy raw material liquid, and naturally cooling to room temperature after casting, to obtain a rare earth alloy high entropy alloy (CoCrFeNi) 100-x G x .
[0045] Step (5), preparing the rare earth alloy high entropy alloy (CoCrFeNi) in step (4) 100-x G x The microstructure and mechanical properties were compared to screen out rare earth alloyed high entropy alloys with both plasticity and strength.
[0046] In this embodiment, two rare earth alloyed high entropy alloys (CoCrFeNi) were finally prepared by the above method. 99 Gd1 alloy and (CoCrFeNi) 97 Gd3 alloy cast button ingot 200g.
[0047] The microstructures of the two rare earth alloyed high entropy alloys were characterized, and the high entropy alloy CoCrFeNi without rare earth alloy was used as a control. Figure 1a to Figure 1c As can be seen from the figure, compared with (CoCrFeNi) 99 Gd1, (CoCrFeNi) 97 The changes in the microstructure of the Gd3 rare earth alloyed high entropy alloy and the CoCrFeNi high entropy alloy are that the grains are significantly refined compared to the matrix CoCrFeNi high entropy alloy without Gd addition, and the microstructure is distributed in a dendrite morphology. This shows that after the addition of Gd, a new Gd-containing rare earth phase is formed, while the matrix FCC phase still exists in large quantities, ensuring the plasticity of the alloy system; the microphase composition of the alloy presents a dendrite phase (DR) and an interdendrite phase (ID), and the microstructure grains are significantly refined; the dendrite phase (DR) is the FCC phase, the interdendrite phase (ID) is the Gd-containing rare earth phase, and the Gd-containing rare earth phase is the HS phase, which has a CaCu5-type hexagonal structure and is a typical strengthening phase.
[0048] This embodiment also tests CoCrFeNi alloy, (CoCrFeNi) 99 Gd1 alloy and (CoCrFeNi) 97 The compressive mechanical properties of Gd3 alloy were tested and the results are as follows Figure 2As shown, in terms of strength, the yield strength of CoCrFeNi alloy is 235MPa, (CoCrFeNi) 99 The yield strength of Gd1 alloy is 380MPa, (CoCrFeNi) 97 The yield strength of Gd3 alloy is 650MPa; in terms of plasticity, the plasticity of CoCrFeNi alloy is above 60%, (CoCrFeNi) 99 The plasticity of Gd1 alloy at fracture is 44%, (CoCrFeNi) 97 The plasticity of Gd3 alloy at fracture is 35%; compared with (CoCrFeNi) 99 Gd1 alloy, (CoCrFeNi) 97 The changes in the mechanical properties of Gd3 alloy and CoCrFeNi alloy show that (CoCrFeNi) 99 Gd1 alloy and (CoCrFeNi) 97 The Gd3 alloy has significantly improved strength compared to the base alloy CoCrFeNi high entropy alloy, while also having good plasticity.
[0049] Example 2
[0050] This embodiment is based on the composition design method of rare earth alloyed high entropy alloy, comprising the following steps:
[0051] Step (1), according to the lattice distortion effect, select a rare earth element with a large difference in atomic radius from the four main elements of the CoCrFeNi high entropy alloy as an additive element to prepare a high entropy alloy having a chemical formula of (CoCrFeNi): 100-x RE x Rare earth alloyed high entropy alloy, RE is a rare earth element;
[0052] Step (2), determine (CoCrFeNi) 100-x La x The contents of the four main elements in the rare earth alloy high entropy alloy meet the standards of the second generation high entropy alloy. In this embodiment, the atomic percentage ratio of the four main elements in the CoCrFeNi high entropy alloy is 1:1:1:1; the rare earth element is lanthanum La;
[0053] Step (3), determine the amount of the added element in the CoCrFeNi high entropy alloy so that the designed (CoCrFeNi) 100-x La x The atomic percentage X value of the medium rare earth element La is 0.05 to 3.0 at.%;
[0054] Step (4), according to the designed (CoCrFeNi) 100-x La xPreparation of rare earth alloyed high entropy alloys with different added elements and rare earth alloyed high entropy alloys with different added elements; rare earth alloyed high entropy alloy (CoCrFeNi) 100-x La x The preparation method is:
[0055] Step (4-1), according to the rare earth alloy high entropy alloy (CoCrFeNi) 100-x La x Prepare alloy raw materials according to the proportion of each element;
[0056] Step (4-2), placing all alloy raw materials into a vacuum arc melting device for melting at the same time to obtain alloy raw material liquid;
[0057] Step (4-3), casting the alloy raw material liquid, and naturally cooling to room temperature after casting, to obtain a rare earth alloy high entropy alloy (CoCrFeNi) 100-x La x .
[0058] Step (5), preparing the rare earth alloy high entropy alloy (CoCrFeNi) in step (4) 100-x La x The microstructure and mechanical properties were compared to screen out rare earth alloyed high entropy alloys with both plasticity and strength.
[0059] In this embodiment, two rare earth alloyed high entropy alloys (CoCrFeNi) were finally prepared by the above method. 99 La1 alloy and (CoCrFeNi) 98 200g of La2 alloy cast button ingot.
[0060] The microstructures of the two rare earth alloyed high entropy alloys were characterized, and the high entropy alloy CoCrFeNi without rare earth alloy was used as a control. Figure 3a to Figure 3c As can be seen from the figure, compared with (CoCrFeNi) 99 La1, (CoCrFeNi) 98The changes in the microstructure of La2 rare earth alloyed high entropy alloy and CoCrFeNi high entropy alloy are that the grains are significantly refined compared to the matrix CoCrFeNi high entropy alloy without La addition, and the microstructure is distributed in a dendrite morphology. This shows that after adding La, a new La-containing rare earth phase is formed, while the matrix FCC phase still exists in large quantities, ensuring the plasticity of the alloy system; the microphase composition of the alloy presents a dendrite phase (DR) and an interdendrite phase (ID), and the microstructure grains are significantly refined; the dendrite phase (DR) is the FCC phase, the interdendrite phase (ID) is the La-containing rare earth phase, and the La-containing rare earth phase is the HS phase, which has a CaCu5-type hexagonal structure and is a typical strengthening phase.
[0061] This embodiment also tests CoCrFeNi alloy, (CoCrFeNi) 99 La1 alloy and (CoCrFeNi) 98 The compressive mechanical properties of La2 alloy were tested and the results are as follows Figure 4 As shown, in terms of strength, the yield strength of CoCrFeNi alloy is 235MPa, (CoCrFeNi) 99 La1 alloy is 490MPa, (CoCrFeNi) 98 La2 alloy is 370MPa; in terms of plasticity, the plasticity of CoCrFeNi alloy is above 60%, (CoCrFeNi) 99 The plasticity of La1 alloy at fracture is 30%, (CoCrFeNi) 98 The plasticity of La2 alloy at fracture is 23%; compared with (CoCrFeNi) 99 La1 alloy, (CoCrFeNi) 98 The changes in the mechanical properties of La2 alloy and CoCrFeNi alloy show that (CoCrFeNi) 99 La1 alloy and (CoCrFeNi) 98 The strength of La2 alloy is significantly improved compared with the base alloy CoCrFeNi high entropy alloy, while also having good plasticity.
[0062] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the claims of this patent application.
Claims
1. A composition design method based on rare earth alloying high entropy alloy, characterized in that: The steps include: Step (1), according to the lattice distortion effect, select a rare earth element with a large difference in atomic radius from the four main elements of the CoCrFeNi high entropy alloy as an additive element to prepare a high entropy alloy having a chemical formula of (CoCrFeNi): 100-x RE x Rare earth alloy high entropy alloy, RE is a rare earth element; rare earth elements whose atomic radius difference with the component elements in CoCrFeNi high entropy alloy is between 40 and 60 pm are defined as rare earth elements with large atomic radius difference; rare earth element lanthanum La is selected as an additive element; Step (2), determine (CoCrFeNi) 100-x RE x The contents of the four main elements in the rare earth alloy high entropy alloy meet the standards of the second generation high entropy alloy; the contents of the four main elements of the CoCrFeNi high entropy alloy are determined as follows: the atomic percentage of cobalt Co is 5 to 35 at.%, the atomic percentage of chromium Cr is 5 to 35 at.%, the atomic percentage of iron Fe is 5 to 35 at.%, and the atomic percentage of nickel Ni is 5 to 35 at.%; Step (3), determine the amount of the added element in the CoCrFeNi high entropy alloy so that the designed (CoCrFeNi) 100-x RE x The atomic percentage X of the medium rare earth element RE is 0.5 at.%, 1.0 at.%, 2.0 at.% or 3.0 at.%; Step (4), according to the designed (CoCrFeNi) 100-x RE x Preparation of rare earth alloyed high entropy alloys with different added elements and rare earth alloyed high entropy alloys with different added elements; Step (5), preparing the rare earth alloy high entropy alloy (CoCrFeNi) in step (4) 100-x RE x The microstructure and mechanical properties were compared to screen out rare earth alloyed high entropy alloys with both plasticity and strength.
2. The composition design method based on rare earth alloyed high entropy alloy according to claim 1, characterized in that: The atomic percentage ratio of the four main elements in the CoCrFeNi high entropy alloy is 1:1:1:
1.
3. The composition design method based on rare earth alloyed high entropy alloy according to claim 1, characterized in that: In step (4), rare earth alloy high entropy alloy (CoCrFeNi) 100-x RE x Prepared by vacuum arc melting; Step (4-1), according to the rare earth alloy high entropy alloy (CoCrFeNi) 100-x RE x The alloy raw materials are prepared according to the proportion of each element in the alloy raw materials; the purity of the alloy raw materials used is greater than or equal to 99.99wt%; Step (4-2), placing the alloy raw material in a vacuum arc melting device for melting to obtain alloy raw material liquid; Step (4-3), casting the alloy raw material liquid, and naturally cooling to room temperature after casting, to obtain a rare earth alloy high entropy alloy (CoCrFeNi) 100-x RE x .