Silicon carbide / rare earth neodymium iron boron composite magnetic material and preparation method thereof
By adding modified silicon carbide fibers to rare earth neodymium iron boron magnetic materials and connecting them with borate coupling agent, a network-like structure is formed, which solves the problem of material brittleness, improves tensile strength and impact resistance, and is suitable for complex environments .
Patent Information
- Application Number
- CN202211292522.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-21
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-10-21
AI Technical Summary
The existing rare earth permanent magnet neodymium iron boron materials are brittle materials, with high strength but low toughness, easy to break, and difficult to meet the mechanical and chemical performance requirements of complex use environments.
Silicon carbide/rare earth neodymium iron boron composite magnetic material is used to mix modified neodymium iron boron powder and modified silicon carbide fibers, and connect it with borate ester coupling agent to form a network structure to enhance the tensile strength and resistance of the material. Impact performance.
It significantly improves the tensile strength and impact resistance of rare earth neodymium iron boron magnetic materials, reduces the brittleness of the material, and makes it have higher strength and toughness in all directions, and is suitable for complex environments.
Smart Images

Figure GDA0005113048120000071 
Figure GDA0005113048120000081
Abstract
Description
Technical Field
[0001] The present application relates to the field of rare earth neodymium iron boron composite magnetic materials, and more specifically, to a silicon carbide / rare earth neodymium iron boron composite magnetic material and a preparation method thereof. Background Art
[0002] Rare earth permanent magnet material refers to an alloy formed by rare earth metals and transition metals. This permanent magnet material made by a certain process has extremely strong magnetism and can maintain it for a long time. This material is now divided into the first, second and third generation rare earth permanent magnet materials. The third generation rare earth permanent magnet NdFeB is the strongest permanent magnet among contemporary magnets. Rare earth NdFeB permanent magnet material has excellent magnetic properties and has been widely used in electronics, power machinery, medical equipment, toys, packaging, hardware machinery, aerospace and other fields.
[0003] In the related art, the main raw materials of rare earth permanent magnet NdFeB include rare earth metal neodymium, metal element iron, non-metallic element boron, and elements such as dysprosium, niobium, aluminum, and copper. Although the application of rare earth NdFeB permanent magnets is mainly to use their magnetic properties, due to the different use environments and conditions, in addition to the magnetic properties, there are also requirements for mechanical properties and chemical properties of the magnets. The existing rare earth permanent magnet NdFeB belongs to a brittle material, and its mechanical properties are hard and brittle, that is, high strength and low toughness, and there is almost no plastic deformation before breaking, that is, it breaks in the elastic deformation stage. Therefore, the preparation of rare earth permanent magnet NdFeB with low brittleness and high toughness is a problem to be solved in the current research on rare earth permanent magnet NdFeB. Summary of the invention
[0004] In order to reduce the brittleness of rare earth permanent magnet NdFeB materials, the present application provides a silicon carbide / rare earth NdFeB composite magnetic material and a preparation method thereof.
[0005] In the first aspect, the present application provides a silicon carbide / rare earth neodymium iron boron composite magnetic material, which adopts the following technical scheme: a silicon carbide / rare earth neodymium iron boron composite magnetic material, comprising the following raw materials in parts by weight: 20-30 parts of modified neodymium iron boron powder and 1-5 parts of modified silicon carbide fiber; the modified neodymium iron boron powder is modified from an acidic aqueous solution, a sodium-containing oxidant aqueous solution and water; the modified silicon carbide fiber is modified from a borate coupling agent and a solvent, and the borate coupling agent accounts for 0.5-1wt% of the modified silicon carbide fiber.
[0006] By adopting the above technical scheme, since the tensile strength of NdFeB magnets is 50-160MPa, the NdFeB magnets prepared from NdFeB powders are brittle and easy to break; while the tensile strength of silicon carbide fibers is 2000-4000MPa, the silicon carbide / rare earth NdFeB composite magnets prepared by mixing NdFeB powders with silicon carbide fibers have greatly improved tensile strength compared to the original NdFeB magnets; however, there is no adhesion between the NdFeB powders and the silicon carbide surfaces, and the tensile strengths differ greatly, therefore, the present application uses modified NdFeB and modified silicon carbide fibers, and the coupling agent of the silicon carbide fibers is selected as a borate coupling agent, so that the borate coupling agent is connected to the silicon carbide fibers while being stably connected to the NdFeB powders containing a large amount of boron; finally, a silicon carbide / rare earth NdFeB composite magnet with higher tensile strength is obtained, thereby reducing the brittleness of the NdFeB magnets.
[0007] Optionally, the NdFeB powder is composed of 60-70 parts of iron, 0.5-1.2 parts of boron, 15-20 parts of praseodymium and neodymium, 10-15 parts of cerium, 1.5-2.5 parts of gadolinium, 0.1-0.5 parts of cobalt, 0.1-0.5 parts of aluminum, 0.1-0.2 parts of copper and 0.2-0.4 parts of zirconium; the above parts are all parts by weight.
[0008] By adopting the above technical solution, the metal used to prepare the above NdFeB powder contains not only the three metals of NdPr, Fe and B, but also metals such as cerium, gadolinium, cobalt, aluminum, copper and zirconium, thereby enhancing the tensile strength of the NdFeB magnet.
[0009] Optionally, the silicon carbide fiber is a silicon carbide fiber with whiskers.
[0010] By adopting the above technical solution, silicon carbide fibers with whiskers can form a network structure in NdFeB powder compared to silicon carbide fibers without whiskers, connect the NdFeB powder into a whole, and enhance the tensile strength of the prepared silicon carbide / rare earth NdFeB composite magnetic material in all directions.
[0011] Optionally, the length of the silicon carbide fiber is 10-50 μm.
[0012] By adopting the above technical solution, silicon carbide fibers with a length of 10-50 μm can just connect the NdFeB powder and form a network structure with other silicon carbide fibers to prepare silicon carbide / rare earth NdFeB composite magnetic materials with high tensile strength.
[0013] Optionally, the sodium-containing oxidant is sodium peroxide or sodium superoxide.
[0014] By adopting the above technical solution, sodium peroxide or sodium superoxide is used as an oxidant, and other non-metallic impurities will not be introduced when oxidizing the NdFeB magnetic material, and the magnetic properties of the NdFeB will not be affected.
[0015] Optionally, the acidic aqueous solution is a hydrochloric acid aqueous solution, a sulfuric acid aqueous solution, a phosphoric acid aqueous solution or a nitric acid aqueous solution.
[0016] By adopting the above technical solution, the acidic aqueous solution can etch grooves and recesses on the outer surface of the NdFeB powder, making the connection between the NdFeB powder and the borate coupling agent more stable, thereby making the connection between the NdFeB powder and the modified silicon carbide fiber more stable.
[0017] In a second aspect, the present application provides a method for preparing a silicon carbide / rare earth neodymium iron boron composite magnetic material, using the following technical solution:
[0018] A method for preparing a silicon carbide / rare earth neodymium iron boron composite magnetic material comprises the following steps:
[0019] Step 1, preparation of modified NdFeB powder: placing the modified NdFeB powder in an acidic aqueous solution, soaking it, and washing it with water; then placing it in an aqueous solution containing a sodium oxidant, soaking it, and washing it with water to obtain the modified NdFeB powder;
[0020] Step 2, preparation of modified silicon carbide fiber: Preparation of modified silicon carbide fiber: Add silicon carbide fiber and borate coupling agent into toluene, stir and react for 3-6 hours under nitrogen protection, the reaction temperature is 70-80°C, after the reaction is completed, filter and discard the filtrate, centrifuge in acetone aqueous solution, and wash in water to obtain modified silicon carbide fiber;
[0021] Step 3, the modified NdFeB powder and the modified SiC fiber mixture are mixed and granulated, and the granulated granules are injection molded into SiC / rare earth NdFeB composite magnetic materials of a desired shape.
[0022] By adopting the above technical scheme, in step 1, the purpose of soaking in the acidic aqueous solution and the oxidant sodium-containing oxidant aqueous solution is to etch the surface of the NdFeB powder, and the purpose of washing with water after each soaking is to avoid the two etching solutions from mixing and reacting with each other, thereby affecting the etching effect; in step 2, under appropriate temperature conditions, the borate coupling agent can be connected to the silicon carbide fiber as much as possible; thereby, the stability of the connection between the modified NdFeB powder and the modified silicon carbide fiber is improved, and the obtained silicon carbide / rare earth NdFeB composite magnetic material has high tensile strength and low brittleness.
[0023] Optionally, in step 1, modified NdFeB powder is prepared by placing the modified NdFeB powder in an acidic aqueous solution, soaking it for 20-30 minutes, and washing it with water; then placing it in an aqueous solution containing a sodium oxidant and soaking it for 15-20 minutes, washing it with water, and drying it to obtain the modified NdFeB powder.
[0024] By adopting the above technical scheme, the NdFeB powder is reacted with the acidic aqueous solution for an appropriate time; and reacted with the sodium-containing oxidant for an appropriate time, the obtained modified NdFeB powder has the best etching effect, the connection between the modified NdFeB powder and the modified carbon fiber is more stable, and the final silicon carbide / rare earth NdFeB composite magnetic material has high tensile strength and low brittleness.
[0025] In summary, this application has the following beneficial effects:
[0026] 1. In the present application, since the tensile strength of NdFeB magnets is 50-160MPa and the tensile strength of silicon carbide fibers is 2000-4000MPa, the tensile strength of silicon carbide / rare earth NdFeB composite magnets obtained by mixing NdFeB powders with silicon carbide fibers will be greatly improved compared to the original NdFeB magnets; while the borate coupling agent connects the silicon carbide fibers, it is stably connected to the NdFeB powders containing a large amount of boron; finally, a silicon carbide / rare earth NdFeB composite magnet with high tensile strength is obtained, thereby reducing the brittleness of the NdFeB magnets;
[0027] 2. The present application preferably uses silicon carbide fibers with whiskers. The purpose is that, compared with silicon carbide fibers without whiskers, silicon carbide fibers with whiskers can form a network structure in the NdFeB powder, connect the NdFeB powder into a whole, and enhance the tensile strength of the prepared silicon carbide / rare earth NdFeB composite magnetic material in all directions;
[0028] 3. In the preparation step 1 of the present application, sodium peroxide or sodium superoxide is preferred. The purpose is that sodium peroxide or sodium superoxide, as an oxidant, will not introduce other non-metallic impurities when oxidizing the NdFeB magnetic material, and will not affect the magnetic properties of NdFeB. DETAILED DESCRIPTION
[0029] The present application is further described in detail below in conjunction with embodiments and comparative examples.
[0030] The sources of raw materials for the following embodiments and comparative examples are provided: the raw materials for the embodiments and comparative examples can be purchased commercially, silicon carbide fibers with whiskers and silicon carbide fibers without whiskers are purchased from Shanghai Maoguo Nano Technology Co., Ltd.; borate coupling agent, model, PEA, is purchased from Jining Huakai Resin Co., Ltd.; silane coupling agent model is KH-550.
[0031] Preparation of NdFeB magnetic powder:
[0032] Raw materials: 66.32kg iron powder, 0.93kg boron powder, 17.4kg praseodymium-neodymium powder, 12kg cerium powder, 3.2kg gadolinium powder, 0.3kg cobalt powder, 0.3kg aluminum powder, 0.3kg zirconium powder, 0.15kg copper powder; the raw materials are sent to the European mill through a bucket elevator for grinding to the required particle size of 50-100μm, and then the powder is selected by a sieving machine and then collected and bagged in a powder collector.
[0033] An embodiment of a silicon carbide / rare earth neodymium iron boron composite magnetic material
[0034] Example 1
[0035] A silicon carbide / rare earth neodymium iron boron composite magnetic material, the preparation steps of which are:
[0036] Step 1, preparation of modified NdFeB powder: 5kg NdFeB powder is placed in a 2wt% hydrochloric acid aqueous solution, the hydrochloric acid aqueous solution completely submerges the NdFeB powder, soaks for 30 minutes, and then rinses in running water for 5 minutes; then placed in a 3wt% sodium peroxide aqueous solution and soaked for 20 minutes, the sodium peroxide aqueous solution completely submerges the NdFeB powder, and after the soaking, rinses in running water for 5 minutes; dried at 70°C for 2 hours to obtain modified NdFeB powder;
[0037] Step 2, preparation of modified silicon carbide fiber: add 1 kg of silicon carbide fiber with whiskers of 30 μm in length and 0.5 wt% of borate coupling agent in silicon carbide fiber to 6 kg of toluene, stir and react at a speed of 100 rpm for 4 hours under nitrogen protection, the reaction temperature is 75°C, after the reaction is completed, vacuum filter, discard the filtrate, disperse the obtained product with 50 wt% acetone aqueous solution, centrifuge at a speed of 1000 rpm for 20 minutes, wash the centrifugal precipitate in running water for 5 minutes; dry at 90°C for 10 hours to obtain modified silicon carbide fiber;
[0038] Step 3, 2kg of modified NdFeB powder and 0.5kg of modified silicon carbide fiber mixture are mixed and granulated. The temperatures of each section of the extruder are 270°C, 270°C, 275°C, 275°C, 280°C, and 280°C, respectively. The rotation speed is 60rpm, the injection molding temperature is 280°C, and the pressure is 40MPa. The granulated pellets are injection molded into silicon carbide / rare earth NdFeB composite magnetic materials of the desired shape.
[0039] Example 2
[0040] The difference from Example 1 is that step 2 is different from step 3;
[0041] Step 2, preparation of modified silicon carbide fiber: add 1 kg of whisker silicon carbide fiber with a length of 30 μm and 1 wt% of borate coupling agent of silicon carbide fiber to 6 kg of toluene, stir and react at a speed of 100 rpm for 4 hours under nitrogen protection, and the reaction temperature is 75°C. After the reaction is completed, vacuum filter and discard the filtrate. Disperse the obtained product with 50 wt% acetone aqueous solution, centrifuge at a speed of 1000 rpm for 20 minutes, wash the centrifugal precipitate in running water for 5 minutes, and dry at 90°C for 10 hours to obtain modified silicon carbide fiber;
[0042] Step 3, 3kg of modified NdFeB powder and 0.1kg of modified silicon carbide fiber mixture are mixed and granulated. The temperatures of each section of the extruder are 270°C, 270°C, 275°C, 275°C, 280°C, and 280°C, respectively. The rotation speed is 60rpm, the injection molding temperature is 280°C, and the pressure is 40MPa. The granulated pellets are injection molded into silicon carbide / rare earth NdFeB composite magnetic materials of the desired shape.
[0043] Example 3
[0044] The difference from Example 1 is that step 2 is different from step 3;
[0045] Step 2, preparation of modified silicon carbide fiber: add 1 kg of silicon carbide fiber with whiskers of 30 μm in length and 0.7 wt% of borate coupling agent in silicon carbide fiber to 6 kg of toluene, stir and react at a speed of 100 rpm for 4 hours under nitrogen protection, the reaction temperature is 75°C, after the reaction is completed, vacuum filter, discard the filtrate, disperse the obtained product with 50 wt% acetone aqueous solution, centrifuge at a speed of 1000 rpm for 20 minutes, wash the centrifugal precipitate in running water for 5 minutes; dry at 90°C for 10 hours to obtain modified silicon carbide fiber;
[0046] Step 3, 2.5 kg of modified NdFeB powder and 0.25 kg of modified silicon carbide fiber mixture are mixed and granulated. The temperatures of each section of the extruder are 270°C, 270°C, 275°C, 275°C, 280°C, and 280°C, respectively. The rotation speed is 60 rpm, the injection molding temperature is 280°C, and the pressure is 40 MPa. The granulated pellets are injection molded into silicon carbide / rare earth NdFeB composite magnetic materials of the desired shape.
[0047] Example 4
[0048] The difference from Example 1 is that the 2 wt % hydrochloric acid aqueous solution in step 1 is replaced by an equal weight of 4 wt % nitric acid aqueous solution.
[0049] Example 5
[0050] The difference from Example 1 is that the 3 wt % sodium peroxide aqueous solution in step 1 is replaced by an equal weight of 3 wt % sodium superoxide aqueous solution.
[0051] Example 6
[0052] The difference from Example 1 is that the 3 wt % sodium peroxide aqueous solution in step 1 is replaced by an equal weight of 3 wt % sodium periodate aqueous solution.
[0053] Example 7
[0054] The difference from Example 1 is that the 30 μm silicon carbide fibers with whiskers in step 2 are replaced with 50 μm silicon carbide fibers with whiskers of the same weight.
[0055] Example 8
[0056] The difference from Example 1 is that the 30 μm silicon carbide fibers with whiskers in step 2 are replaced with 10 μm silicon carbide fibers with whiskers of the same weight.
[0057] Example 9
[0058] The difference from Example 1 is that the whisker-containing silicon carbide fibers with a length of 30 μm in step 2 are replaced by whisker-free silicon carbide fibers with a length of 30 μm of the same weight.
[0059] Comparative Example 1
[0060] The difference from Example 1 is that modified NdFeB powder is not used;
[0061] Step 1, preparation of modified silicon carbide fiber: add 1 kg of silicon carbide fiber with whiskers of 30 μm in length and 0.5 wt% of borate coupling agent in silicon carbide fiber to 6 kg of toluene, stir and react at a speed of 100 rpm for 4 hours under nitrogen protection, the reaction temperature is 75°C, after the reaction is completed, vacuum filter, discard the filtrate, disperse the obtained product with 50 wt% acetone aqueous solution, centrifuge at a speed of 1000 rpm for 20 minutes, wash the centrifugal precipitate in running water for 5 minutes; dry at 90°C for 10 hours to obtain modified silicon carbide fiber;
[0062] Step 3, 2kg of NdFeB powder and 0.5kg of modified silicon carbide fiber mixture are mixed and granulated, the temperatures of each section of the extruder are 270℃, 270℃, 275℃, 275℃, 280℃, 280℃, the speed is 60rpm, the injection molding temperature is 280℃, the pressure is 40MPa, and the granulated pellets are injection molded into silicon carbide / rare earth NdFeB composite magnetic materials of the required shape.
[0063] Comparative Example 2
[0064] The difference from Example 1 is that the pickling step is not performed in step 1;
[0065] Step 1, preparation of modified NdFeB powder: soak 5 kg NdFeB powder in 3 wt % sodium peroxide aqueous solution for 50 min, completely submerge the NdFeB powder in the sodium peroxide aqueous solution, wash in running water for 5 min after soaking; dry at 70°C for 2 h to obtain modified NdFeB powder.
[0066] Comparative Example 3
[0067] The difference from Example 1 is that no oxidizing step with an oxidant is performed in step 1;
[0068] Step 1, preparation of modified NdFeB powder: 5 kg of NdFeB powder is placed in a 2 wt % hydrochloric acid aqueous solution, the hydrochloric acid aqueous solution completely submerges the NdFeB powder, soaks for 50 minutes, and then washes in running water for 5 minutes; and dries at 70° C. for 2 hours to obtain modified NdFeB powder.
[0069] Comparative Example 4
[0070] The difference from Example 1 is that no water washing step is performed in step 1;
[0071] Step 1, preparation of modified NdFeB powder: place 5kg of NdFeB powder in a 2wt% hydrochloric acid aqueous solution, the hydrochloric acid aqueous solution completely submerges the NdFeB powder, and soak for 30 minutes; then place in a 3wt% sodium peroxide aqueous solution and soak for 20 minutes, the sodium peroxide aqueous solution completely submerges the NdFeB powder, after the soaking is completed; dry at 70°C for 2h to obtain modified NdFeB powder.
[0072] Comparative Example 5
[0073] The difference from Example 1 is that the borate coupling agent in step 2 is replaced by an equal weight of a silane coupling agent.
[0074] Comparative Example 6
[0075] The difference from Example 1 is that the borate coupling agent accounting for 0.5 wt % of the silicon carbide fiber in step 2 is replaced by an equal weight of borate coupling agent accounting for 0.05 wt % of the silicon carbide fiber.
[0076] Comparative Example 7
[0077] The difference from Example 1 is that the borate coupling agent accounting for 0.5 wt % of the silicon carbide fiber in step 2 is replaced by an equal weight of borate coupling agent accounting for 5 wt % of the silicon carbide fiber.
[0078] Comparative Example 8
[0079] The difference from Example 1 is that the whisker-containing silicon carbide fibers with a length of 30 μm in step 2 are replaced by polyurethane fibers with a length of 30 μm of the same weight.
[0080] Comparative Example 9
[0081] The difference from Example 1 is that the 30 μm silicon carbide fibers with whiskers in step 2 are replaced with 100 μm silicon carbide fibers with whiskers of the same weight.
[0082] Comparative Example 10
[0083] Commercially available NdFeB rare earth magnetic material is used; model: N35; manufacturer: Ningbo Xinhao Magnetic Material Co., Ltd.
[0084] Performance testing
[0085] The silicon carbide / rare earth neodymium iron boron composite magnetic materials prepared in Examples 1 to 9 and Comparative Examples 1 to 10 were used for performance testing to detect the residual magnetic induction intensity, the maximum magnetic energy product and the tensile strength; the detection basis of the residual magnetic induction intensity and the maximum magnetic energy product is GB / T3217 permanent magnetic (hard magnetic) material magnetic test method; the tensile strength test is based on GB / T228.1-2021 "Metallic Material Tensile Test Part 1: Room Temperature Test Method"; the impact strength test is based on the inspection of the GB / T3808-2002 pendulum impact tester; the test results are shown in Table 1 below;
[0086] Table 1
[0087]
[0088]
[0089] In combination with Examples 1, 2 and 3, it can be seen that when the modification method and addition ratio of the modified silicon carbide fiber and the modified neodymium iron boron fiber are within the protection scope of this application, the obtained silicon carbide / rare earth neodymium iron boron composite magnetic material has high tensile strength, increased impact strength, low brittleness and is not easy to break during collision.
[0090] Combining Example 1 with Example 4, it can be seen that when the hydrochloric acid in step 1 is replaced by nitric acid, the tensile strength and impact strength of the silicon carbide / rare earth neodymium iron boron composite magnetic material finally prepared in Example 1 and Example 4 are not much different. Therefore, the modification with nitric acid or hydrochloric acid does not have a great influence on the modification effect of silicon carbide fiber.
[0091] Combining Example 1 with Examples 5 and 6, it can be seen that when the sodium peroxide in step 1 of Example 1 is replaced with sodium superoxide, the tensile strength and impact strength of the silicon carbide / rare earth neodymium iron boron composite magnetic material finally prepared in Example 1 and Example 5 are not much different, and the brittleness is low and it is not easy to break during collision. Therefore, the use of sodium peroxide or sodium superoxide does not have a great effect on the modification effect of silicon carbide fiber. In Example 6, sodium periodate is used. Although the tensile strength and impact strength of the silicon carbide / rare earth neodymium iron boron composite magnetic material prepared are also large, they are not as good as those in Example 1 and Example 4. The reason is that non-metallic ions iodine ions are introduced into sodium periodate, and the introduction of sodium periodate reduces the magnetism of the silicon carbide / rare earth neodymium iron boron composite magnetic material.
[0092] In combination with Example 1 and Examples 7 and 8, and Comparative Example 9, it can be seen that the lengths of the whiskered silicon carbide fibers used in Step 2 of Examples 1, 7, and 8 are 30 μm, 50 μm, and 10 μm, respectively, and the tensile strength and impact strength of the silicon carbide / rare earth NdFeB composite magnetic materials obtained in Examples 1, 7, and 8 are both relatively large, proving that when the length of the whiskered silicon carbide fibers is within the protection scope of the present application, the silicon carbide / rare earth NdFeB composite magnetic materials obtained have low brittleness and are not easily broken by collision. However, the length of the whiskered silicon carbide fibers in Comparative Example 9 is 100 μm, and the tensile strength and impact strength of the silicon carbide / rare earth NdFeB composite magnetic materials obtained are relatively low, proving that in the present application, when the length of the silicon carbide fibers is within the range of 10-50 μm, the silicon carbide / rare earth NdFeB composite magnetic materials obtained have low brittleness and are not easily broken by collision.
[0093] In combination with Example 1 and Comparative Examples 1, 2, 3, and 4, it can be seen that Comparative Example 1 does not undergo pickling, water washing, oxidation, or water washing; Comparative Example 2 does not undergo pickling; Comparative Example 3 does not undergo oxidation; and Comparative Example 4 does not undergo water washing. The tensile strength and impact strength of the obtained silicon carbide / rare earth NdFeB composite magnetic material are relatively low, proving that each step in the processing method of the NdFeB magnetic material in step 1 of the present application is indispensable.
[0094] In combination with Examples 1, 9 and Comparative Example 8, it can be seen that Example 9 uses whisker-free silicon carbide fibers, and the tensile strength and impact strength of the silicon carbide / rare earth neodymium iron boron composite magnetic material obtained are lower than those of Example 1; Comparative Example 8 uses polyurethane fibers, and the tensile strength and impact strength of the silicon carbide / rare earth neodymium iron boron composite magnetic material obtained are lower; this proves that silicon carbide fibers with whiskers are preferred in the preparation of the raw materials of the present application.
[0095] Combining Example 1 and Comparative Example 5, it can be seen that the tensile strength and impact strength of the silicon carbide / rare earth neodymium iron boron composite magnetic material prepared by using a silane coupling agent in step 2 of Comparative Example 5 are relatively low, which proves that a borate coupling agent must be used in the preparation of raw materials in this application.
[0096] Combining Examples 1, 2, 3 with Comparative Examples 6 and 7, it can be seen that in Examples 1, 2, and 3, the amount of borate coupling agent added is 0.5wt%, 1wt% and 0.7wt% of the whisker silicon carbide fiber, respectively, and the tensile strength and impact strength of the prepared silicon carbide / rare earth neodymium iron boron composite magnetic material are relatively high; while in Comparative Examples 6 and 7, the amount of borate coupling agent added is 0.05wt% and 5wt% of the whisker silicon carbide fiber, respectively, and the tensile strength and impact strength of the prepared silicon carbide / rare earth neodymium iron boron composite magnetic material are relatively low; This proves that the amount of borate coupling agent added is very important when preparing the modified silicon carbide fiber in the present application.
[0097] Combining Example 1 with Comparative Example 10, it can be seen that Comparative Example 10 is a commercially available NdFeB rare earth magnetic material, and the tensile strength of the silicon carbide / rare earth NdFeB composite magnetic material prepared in Example 1 is 2-3 times that of the commercially available NdFeB rare earth magnetic material of Comparative Example 10, and the impact strength is greatly increased, indicating that the silicon carbide / rare earth NdFeB composite magnetic material prepared in the present application has the advantages of high tensile strength and not easy to break.
[0098] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A silicon carbide / rare earth neodymium iron boron composite magnetic material, characterized in that: The invention comprises the following raw materials in parts by weight: 20-30 parts of modified NdFeB powder and 1-5 parts of modified silicon carbide fiber; the modified NdFeB powder is modified by an acidic aqueous solution, a sodium-containing oxidant aqueous solution and water; the modified silicon carbide fiber is modified by a borate coupling agent and a solvent, and the borate coupling agent accounts for 0.5-1wt% of the modified silicon carbide fiber.
2. The silicon carbide / rare earth neodymium iron boron composite magnetic material according to claim 1, characterized in that: The NdFeB powder is composed of 60-70 parts of iron, 0.5-1.2 parts of boron, 15-20 parts of praseodymium and neodymium, 10-15 parts of cerium, 1.5-2.5 parts of gadolinium, 0.1-0.5 parts of cobalt, 0.1-0.5 parts of aluminum, 0.1-0.2 parts of copper and 0.2-0.4 parts of zirconium; the above parts are all parts by weight.
3. The silicon carbide / rare earth neodymium iron boron composite magnetic material according to claim 1, characterized in that: The silicon carbide fiber is a silicon carbide fiber with whiskers.
4. The silicon carbide / rare earth neodymium iron boron composite magnetic material according to claim 1, characterized in that: The length of the silicon carbide fiber is 10-50 μm.
5. The silicon carbide / rare earth neodymium iron boron composite magnetic material according to claim 1, characterized in that: The sodium-containing oxidant is sodium peroxide or sodium superoxide.
6. The silicon carbide / rare earth neodymium iron boron composite magnetic material according to claim 1, characterized in that: The acidic aqueous solution is a hydrochloric acid aqueous solution, a sulfuric acid aqueous solution, a phosphoric acid aqueous solution or a nitric acid aqueous solution.
7. A method for preparing the silicon carbide / rare earth neodymium iron boron composite magnetic material according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1, preparation of modified NdFeB powder: placing the modified NdFeB powder in an acidic aqueous solution, soaking it, and washing it with water; then placing it in an aqueous solution containing a sodium oxidant, soaking it, and washing it with water to obtain the modified NdFeB powder; Step 2, preparation of modified silicon carbide fiber: adding silicon carbide fiber and borate coupling agent into toluene, stirring and reacting for 3-6 hours under nitrogen protection, the reaction temperature is 70-80°C, after the reaction is completed, filtering and discarding the filtrate, centrifuging in acetone aqueous solution, and washing in water to obtain modified silicon carbide fiber; Step 3, the modified NdFeB powder and the modified SiC fiber mixture are mixed and granulated, and the granulated granules are injection molded into SiC / rare earth NdFeB composite magnetic materials of a desired shape.
8. The method for preparing a silicon carbide / rare earth neodymium iron boron composite magnetic material according to claim 7, characterized in that: The step 1, preparation of modified NdFeB powder: placing the modified NdFeB powder in an acidic aqueous solution, soaking for 20-30 minutes, washing with water; then placing the modified NdFeB powder in an aqueous solution containing a sodium oxidant, soaking for 15-20 minutes, washing with water, and drying to obtain the modified NdFeB powder.