A nano twinned silver material and preparation method thereof

The preparation of high-density nanotwin silver material through magnetron sputtering technology solves the problems of low strength and electromigration failure in electronic packaging, and achieves high-strength, electromigration resistance and high thermal stability, which is suitable for high-density, High reliability package.

CN116770247BActive Publication Date: 2024-11-26HARBIN INSTITUTE OF TECHNOLOGY (SHENZHEN) (INSTITUTE OF SCIENCE AND TECHNOLOGY INNOVATION HARBIN INSTITUTE OF TECHNOLOGY SHENZHEN)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310758841.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-26
Publication Date
2024-11-26
Estimated Expiration
2043-06-26

AI Technical Summary

Technical Problem

The application of metal silver in the field of electronic packaging interconnection is limited by its low strength and prone to electromigration failure, and it is difficult to meet the needs of high-density and high-reliability packaging.

Method used

The nano-twin silver material is prepared by magnetron sputtering technology. By applying negative bias voltage on the substrate, a high-density nano-twin silver material is obtained. The proportion of the twin boundary of the material can be improved. The strength and resistance to electromigration of the material while maintaining the conductivity of the thermal conductivity.

Benefits of technology

The high strength, electromigration resistance and high thermal stability of nanotwin silver materials have been achieved, and the problems of low shear strength and poor electromigration resistance of silver interconnection layers have been solved, and the service temperature and reliability of interconnection welding joints have been improved. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116770247B_ABST
    Figure CN116770247B_ABST
Patent Text Reader

Abstract

The present invention provides a nano twin silver material and a preparation method thereof, the preparation method comprising the following steps: step S1, cleaning and drying the substrate; step S2, selecting a silver target as the target material, placing the substrate and the target material in a magnetron sputtering device, and after evacuation, applying a negative bias voltage to the substrate for DC magnetron sputtering deposition, wherein the substrate bias voltage is ‑50-‑200V, the substrate temperature is 25-50°C, the argon gas flow rate is 30-50sccm, the sputtering chamber vacuum is 0.3-1.0Pa, and the deposition time is 15-90min. The technical solution of the present invention is adopted to prepare a nano twin silver material having a high density of nano twins, with a twin boundary ratio of >90%, and under the condition of both high electrical conductivity and high thermal conductivity, the hardness, anti-electromigration performance and thermal stability of the material are improved; the obtained nano twin silver material has excellent comprehensive performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of advanced preparation of metal materials, and in particular relates to a nano twinned silver material and a preparation method thereof. Background Art

[0002] As packaging technology gradually develops towards high density and high reliability, packaging technology requires interconnection materials to have a series of excellent properties such as high strength, good thermal conductivity, thermal stability, resistance to electromigration, and high temperature service. As a metal with excellent electrical and thermal conductivity and anti-oxidation properties, silver is one of the key materials for achieving electrical interconnection in electronic circuit manufacturing. However, the low strength of metallic silver itself and the problem of electromigration failure during service as an interconnection material have severely limited its application in the field of electronic packaging interconnection. Summary of the invention

[0003] In response to the above technical problems, the present invention discloses a nano-twinned silver material and a preparation method thereof. The obtained silver material has excellent properties such as high strength, anti-electromigration performance, high thermal stability, and high thermal and electrical conductivity.

[0004] To this end, the technical solution adopted by the present invention is:

[0005] A method for preparing a nano twinned silver material comprises the following steps:

[0006] Step S1, cleaning and drying the substrate;

[0007] Step S2, a silver target is selected as the target material, and the substrate and the target material are placed in a magnetron sputtering device. After vacuuming, a negative bias voltage is applied to the substrate for DC magnetron sputtering deposition, wherein the substrate bias voltage is -50 to -200 V, the substrate temperature is 25 to 50°C, the argon gas flow rate is 30 to 50 sccm, the vacuum degree of the sputtering chamber is 0.3 to 1.0 Pa, and the deposition time is 15 to 90 min.

[0008] The nano-twin silver material obtained by this technical solution has a high density and can have higher strength and good anti-electromigration performance while maintaining the electrical and thermal conductivity of the silver material itself. Since the grain boundary energy of the coherent nano-twin boundaries is low, only about 10% of the large-angle grain boundaries, the nano-twins in the material can also effectively improve the thermal stability of the material at high temperatures. This high-density nano-twin silver is expected to solve the problems of low shear strength and poor anti-electromigration performance of the silver interconnect layer as an interconnect material, and improve the service temperature and reliability of the interconnect solder joints.

[0009] As a further improvement of the present invention, in step S2, the power is 100-300W.

[0010] As a further improvement of the present invention, the target material is a 99.999% silver target.

[0011] As a further improvement of the present invention, in step S2, the distance between the substrate and the target is 10-20 cm.

[0012] As a further improvement of the present invention, the substrate is a silicon substrate or a copper substrate.

[0013] As a further improvement of the present invention, the thickness of the substrate is 200-500 μm.

[0014] As a further improvement of the present invention, step S1 includes cleaning the polished substrate with an acid solution, then cleaning with deionized water, drying after drying the surface moisture.

[0015] The present invention also discloses a nano twinned silver material, which is prepared by using any one of the above methods for preparing the nano twinned silver material.

[0016] As a further improvement of the present invention, the internal microstructure of the nano-twin silver material is composed of columnar crystals with a width of 200 to 1000 nm that grow along the deposition direction, and the nano-twin lamellae perpendicular to the deposition direction are located inside the columnar crystals, and the average thickness of the nano-twin lamellae is 10-100 nm.

[0017] As a further improvement of the present invention, the columnar crystal surface has a (111) preferred orientation.

[0018] As a further improvement of the present invention, the thickness of the nano-twinned silver material is 2-50 μm.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] First, by adopting the technical solution of the present invention, the nano-twinned silver material prepared has a high density of nano-twins, and the proportion of twin boundaries is >90%. Under the conditions of high electrical conductivity and high thermal conductivity, the hardness, anti-electromigration performance and thermal stability of the material are greatly improved; the obtained nano-twinned silver material has excellent comprehensive performance, can solve the current problems of low strength and poor anti-electromigration performance of silver materials, and can be used as an interconnect layer in power device packaging, advanced packaging, electromechanical system (MEMS) packaging and other fields.

[0021] Second, the technical solution of the present invention adopts magnetron sputtering technology to prepare nano-twin silver materials, which have the advantages of easy control of thickness and uniform structure, and strong adhesion; at the same time, the physical vapor deposition technology is compatible with microelectronics manufacturing processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1This is a focused ion beam (FIB) imaging picture of the cross section of the nano-twin silver material deposited on the silicon substrate in Example 1 of the present invention.

[0023] Figure 2 This is a transmission electron microscope image of the nano-twinned silver material deposited on the silicon substrate in Example 1 of the present invention, showing a high-density nano-twinned layer perpendicular to the deposition direction, and the arrow indicates the deposition direction of the material.

[0024] Figure 3 This is a focused ion beam (FIB) imaging picture of the cross section of the silver material deposited on the silicon substrate in Comparative Example 1 of the present invention.

[0025] Figure 4 This is a FIB imaging picture of the nano-twinned silver material deposited on the silicon substrate in Example 3 of the present invention.

[0026] Figure 5 This is a FIB imaging picture of the nano-twinned silver material deposited on the silicon substrate according to Example 4 of the present invention. DETAILED DESCRIPTION

[0027] The preferred embodiments of the present invention are described in further detail below.

[0028] Example 1

[0029] Using bias DC magnetron sputtering technology <111> Preparation of high-density nanocrystalline silver material on a single crystal silicon substrate. The method for preparing nano-twinned silver material using magnetron sputtering technology described in this embodiment comprises the following steps:

[0030] S1. Use hydrofluoric acid: water solution with a mass ratio of 1:50 to chemically mechanically polish the 2-inch <100> The monocrystalline silicon substrate is cleaned to remove the natural oxide layer; then, it is cleaned with deionized water; and the surface moisture is dried with a spin dryer and then dried for use;

[0031] S2. Place the silicon substrate with the surface oxide film removed and the 99.999% silver target into the magnetron sputtering workbench, and adjust the distance between the substrate and the target to 15 cm;

[0032] S3. After vacuuming, the process parameters of sputtering deposition are set as follows: -100 V bias voltage is applied to the deposition substrate, power: 250 W, substrate temperature: 25° C., argon gas flow rate: 40 sccm, sputtering chamber vacuum: 0.5 Pa, and then sputtering deposition is performed on the substrate;

[0033] S4. Keep step S3 for 20 minutes to obtain a high-density nano-twinned silver material with a thickness of about 3 μm.

[0034] Figure 1They are focused ion beam (FIB) imaging pictures of the cross section of the nano-twin silver material deposited on the silicon substrate in Example 1 of the present invention. It can be seen from the pictures that almost all the grains in the columnar crystals of the material contain high-density nano-twins, and the grains with high-density nano-twins account for about 100%. Figure 2 This is a transmission electron microscope (TEM) image of nanotwinned silver material deposited on a silicon substrate, in which the nanotwins can be clearly seen.

[0035] Example 2

[0036] A high-density nanocrystalline silver material is prepared on a polycrystalline copper substrate using bias DC magnetron sputtering technology. The method for preparing a nano-twinned silver material using magnetron sputtering technology described in this embodiment includes the following steps:

[0037] S1, using 5% (mass percentage) citric acid aqueous solution to clean the polycrystalline copper substrate after mechanical polishing, and using deionized water to clean it; and then using a spin dryer to dry the surface moisture and then dry it for use;

[0038] S2. Place the polycrystalline copper substrate with the surface oxide film removed and the 99.999% silver target into the magnetron sputtering workbench, and adjust the distance between the substrate and the target to 20 cm;

[0039] S3. After vacuuming, the process parameters of sputtering deposition are set as follows: -100 V bias voltage is applied to the deposition substrate, power: 300 W, substrate temperature: 25° C., argon gas flow rate: 50 sccm, sputtering chamber vacuum: 0.5 Pa, and then sputtering deposition is performed on the substrate;

[0040] S4. Keep step S3 for 30 minutes to obtain a high-density nano-twinned silver material with a thickness of about 10 μm.

[0041] Comparative Example 1

[0042] This comparative example comprises the following steps:

[0043] S1, using hydrofluoric acid: water <1:50 solution to chemically mechanically polish the 2-inch <100> The monocrystalline silicon substrate is cleaned to remove the natural oxide layer; then, it is cleaned with deionized water; and the surface moisture is dried with a spin dryer and then dried for use;

[0044] S2. Place the silicon substrate with the surface oxide film removed and the 99.999% silver target into the magnetron sputtering workbench, and adjust the distance between the substrate and the target to 15 cm;

[0045] S3. After vacuuming, the process parameters of sputtering deposition are set as follows: no bias is applied to the deposition substrate, power: 250 W, substrate temperature: 25° C., argon gas flow rate: 40 sccm, sputtering chamber vacuum: 0.5 Pa, and then sputtering deposition is performed on the substrate;

[0046] S4, maintaining step S3 for 20 minutes, and obtaining a nano silver material with a thickness of about 3 μm.

[0047] Figure 3 This is a focused ion beam (FIB) imaging picture of the cross section of the nanotwin silver material deposited on the silicon substrate in Comparative Example 3. From the microstructure, it can be found that under the condition of not applying negative bias, the bottom of the deposited material is an equiaxed crystal transition layer, and nanotwins exist only in a few grains, and no high-density nanotwin material is obtained.

[0048] Example 3

[0049] Using bias DC magnetron sputtering technology <111> Preparation of high-density nanocrystalline silver material on a single crystal silicon substrate. The method for preparing nano-twinned silver material using magnetron sputtering technology described in this embodiment comprises the following steps:

[0050] S1. Use hydrofluoric acid: water solution with a mass ratio of 1:50 to chemically mechanically polish the 2-inch <100> The monocrystalline silicon substrate is cleaned to remove the natural oxide layer; then, it is cleaned with deionized water; and the surface moisture is dried with a spin dryer and then dried for use;

[0051] S2. Place the silicon substrate with the surface oxide film removed and the 99.999% silver target into the magnetron sputtering workbench, and adjust the distance between the substrate and the target to 15 cm;

[0052] S3. After vacuuming, the process parameters of sputtering deposition are set as follows: -50V bias voltage is applied to the deposition substrate, power: 250W, substrate temperature: 25°C, argon gas flow rate: 40sccm, sputtering chamber vacuum: 0.5Pa, and then sputtering deposition is performed on the substrate;

[0053] S4. Keep step S3 for 20 minutes to obtain a high-density nano-twinned silver material with a thickness of about 3 μm.

[0054] Figure 4 This is a FIB imaging picture of the nano-twinned silver material deposited on a silicon substrate under the condition of a substrate bias of -50 V in Example 4. It can be seen from the figure that there is an equiaxed crystal transition layer at the bottom of the material obtained under this condition, and the volume fraction of grains with high-density nano-twins is about 50%.

[0055] Example 4

[0056] Using bias DC magnetron sputtering technology <111> Preparation of high-density nanocrystalline silver material on a single crystal silicon substrate. The method for preparing nano-twinned silver material using magnetron sputtering technology described in this embodiment comprises the following steps:

[0057] S1. Use hydrofluoric acid: water solution with a mass ratio of 1:50 to chemically mechanically polish the 2-inch <100> The monocrystalline silicon substrate is cleaned to remove the natural oxide layer; then, it is cleaned with deionized water; and the surface moisture is dried with a spin dryer and then dried for use;

[0058] S2. Place the silicon substrate with the surface oxide film removed and the 99.999% silver target into the magnetron sputtering workbench, and adjust the distance between the substrate and the target to 15 cm;

[0059] S3. After vacuuming, the process parameters of sputtering deposition are set as follows: -200V bias voltage is applied to the deposition substrate, power: 250W, substrate temperature: 25°C, argon gas flow rate: 40sccm, sputtering chamber vacuum: 0.5Pa, and then sputtering deposition is performed on the substrate;

[0060] S4. Keep step S3 for 20 minutes to obtain a high-density nano-twinned silver material with a thickness of about 3 μm.

[0061] Figure 5 This is a FIB imaging picture of the nano-twinned silver material deposited on the silicon substrate under the condition of a substrate bias of -200 V in Example 5. It can be seen from the figure that high-density nano-twinned silver material can also be obtained under this condition.

[0062] The hardness of the magnetron sputtering Ag materials of Examples 1-4 and Comparative Example 1 was tested using a nanohardness tester, and the results are shown in Table 1. It can be seen that the hardness of the Ag material of Comparative Example 1 with a lower twin density is 0.88 GPa, and the hardness of Example 1 with a high-density twin (90%-Nt) is 1.95 GPa, which is 2.21 times that of Comparative Example 1.

[0063] Table 1. Nanohardness test results of examples and comparative examples

[0064] Material Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Hardness / GPa 1.95 1.86 1.43 1.69 0.88

[0065] The magnetron sputtered Ag materials of Examples 1-4 and Comparative Example 1 were kept at different temperatures for 1 hour to test the thermal stability of the materials, and the critical temperature at which the materials began to detwin and grain growth occurred was determined to evaluate the thermal stability of the materials. The critical temperature at which the materials detwin is formed is shown in Table 2. Compared with 200°C of the material of Comparative Example 1, the instability temperature of the high-density twinned Ag material of the embodiment is increased to 350°C.

[0066] Table 2 Thermal stability test results of the embodiments and comparative examples

[0067] Material Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Instability temperature / ℃ 350 350 300 300 200

[0068] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A method for preparing a nano twinned silver material, characterized in that: The steps include: Step S1, cleaning and drying the substrate; In step S2, a 99.999% silver target is selected as the target material, and the substrate and the target material are placed in a magnetron sputtering device. After vacuuming, a negative bias is applied to the substrate for DC magnetron sputtering deposition, wherein the power is 250 W, the distance between the substrate and the target material is 15 cm, the substrate bias is -100 V, the substrate temperature is 25 ° C, the argon gas flow rate is 40 sccm, the vacuum degree of the sputtering chamber is 0.5 Pa, and the deposition time is 15-90 min.

2. The method for preparing the nano twinned silver material according to claim 1, characterized in that: The substrate is a silicon substrate or a copper substrate.

3. The method for preparing the nano twinned silver material according to claim 2, characterized in that: The thickness of the substrate is 200-500 μm.

4. The method for preparing the nano twinned silver material according to claim 1, characterized in that: Step S1 includes cleaning the polished substrate with an acid solution, then cleaning with deionized water, drying after drying the surface moisture.