An insulating material for synthesizing polycrystalline composite materials and a preparation method thereof
By using insulating materials composed of sodium chloride, magnesium oxide and zirconia to adjust their mass fraction and particle size, the deformation and defects during the sintering process of polycrystalline composite materials are solved, and the product pass rate and sintering uniformity are improved.
Patent Information
- Application Number
- CN202310776341.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-28
AI Technical Summary
In the synthesis process of polycrystalline composite materials, when sodium chloride is used as the insulating material, it is easy to cause deformation, cracks, layering and carbonization of the sintered product, resulting in a low pass rate of the finished product.
Using an insulating material composed of sodium chloride, magnesium oxide and zirconia, by adjusting its mass fraction and particle size, a better melting state and a uniform temperature and pressure field are formed. Magnesium oxide and zirconia serve as support and suppress melting. The role of logistics flow ensures uniformity of the sintering process.
It effectively reduces the deformation and defects of polycrystalline composite materials during sintering, improves the product's pass rate, and ensures the uniform distribution of pressure and temperature fields.
Smart Images

Figure BDA0004309553550000061 
Figure BDA0004309553550000071
Abstract
Description
Technical Field
[0001] The invention relates to an insulating material for synthesizing a polycrystalline composite material and a preparation method thereof, belonging to the technical field of superhard material synthesis. Background Art
[0002] Polycrystalline composite materials, including polycrystalline diamond composite sheets and polycrystalline cubic boron nitride composite sheets, have excellent performance and are widely used in geological exploration and finishing fields. When preparing polycrystalline composite materials, it is necessary to first provide a synthesis block, which includes a synthesis cavity. The synthesis cavity is generally cylindrical. The synthesis cavity is used to place the polycrystalline composite blank. Since the synthesis cavity adopts an indirect heating method, a conductive and heat-generating carbon material is usually used as a heat source. In order to avoid the current passing through the composite sheet and forming a path, the synthesis cavity needs to be isolated from the heat source located at the periphery, top and bottom of the synthesis cavity. Therefore, an insulating medium needs to be set at the periphery, top and bottom of the synthesis cavity. The insulating medium set at the periphery of the synthesis cavity is generally tubular, and the insulating medium set at the top and bottom of the synthesis cavity is generally cylindrical. The chemical composition of the insulating medium is usually sodium chloride, which is not only low in cost, but also has a small internal friction coefficient and good fluidity at high temperatures, so it is widely used in the synthesis of polycrystalline composite materials. However, as the application of polycrystalline composite materials becomes more and more extensive, the industry generally chooses large cavities and multi-piece assembly to improve the production efficiency of polycrystalline composite materials. When assembling large cavities and multi-pieces, the synthesis pressure generally used is relatively high. The sodium chloride under high temperature and high pressure is in a molten state. The molten sodium chloride will flow in the high temperature and high pressure synthesis cavity, causing uneven pressure distribution and uneven temperature field distribution in the synthesis cavity, resulting in deformation, cracks, delamination and carbonization of the sintered polycrystalline composite materials, thereby reducing the performance of the polycrystalline composite materials and the qualified rate of finished products. Summary of the invention
[0003] The purpose of the present invention is to provide an insulating material for synthesizing polycrystalline composite materials, which can solve the problem that the polycrystalline composite materials obtained by sintering are easily deformed when sodium chloride is used as the insulating material for synthesizing polycrystalline composite materials.
[0004] Another object of the present invention is to provide a method for preparing an insulating material for synthesizing polycrystalline composite materials, which can solve the problem of low finished product qualification rate when preparing polycrystalline composite materials with the insulating material currently prepared for synthesizing polycrystalline composite materials.
[0005] In order to achieve the above objectives, the technical solution adopted by the insulating material for synthesizing polycrystalline composite materials of the present invention is:
[0006] An insulating material for synthesizing a polycrystalline composite material mainly consists of sodium chloride, magnesium oxide and zirconium oxide, wherein the mass fraction of the sodium chloride is not less than 50%, the mass fraction of the magnesium oxide is not less than 1%, the mass fraction of the zirconium oxide is not less than 1%, the particle size of the sodium chloride is not less than 100 meshes, the particle size of the magnesium oxide is not less than 200 meshes, and the particle size of the zirconium oxide is not less than 200 meshes.
[0007] The insulating material for synthesizing polycrystalline composite materials of the present invention is mainly composed of sodium chloride, magnesium oxide and zirconium oxide. When the insulating material for synthesizing polycrystalline composite materials of the present invention is used as an insulating sheet for preparing polycrystalline composite materials, during the sintering process (the sintering temperature is generally 1300-1500°C and the pressure is 5-8Gpa, and magnesium oxide and zirconium oxide will not melt at this temperature and pressure), sodium chloride can form a good molten state in the synthesis cavity, which is conducive to the uniform formation of the temperature field; magnesium oxide has high fire-resistant insulation and good thermal conductivity, and will not melt during sintering, and can play a role in supporting and inhibiting the flow of molten materials in the insulating sheet, thereby effectively reducing the deformation of the polycrystalline composite material during sintering; zirconium oxide also has high fire-resistant insulation and good thermal conductivity, and zirconium oxide has good pressure transmission performance, which is conducive to the transmission of pressure and temperature in the cavity, and can ensure that the polycrystalline composite material is uniformly pressurized and heated during the sintering process, and improve the uniformity of the pressure field and temperature field distribution. When the insulating material for synthesizing polycrystalline composite materials of the present invention is used as an insulating sheet for preparing polycrystalline composite materials, the prepared polycrystalline composite materials are not prone to deformation, cracks, delamination and carbonization, and the qualified rate of products can be effectively improved.
[0008] Preferably, among all the sodium chloride particles, the mass fraction of the sodium chloride particles with a particle size of 100 to 200 mesh is not less than 50%. The sodium chloride particles with larger particle size are selected for use in combination with the magnesium oxide and zirconium oxide particles with smaller particle size, so that the magnesium oxide and zirconium oxide particles can wrap the sodium chloride particles. When used as an insulating sheet for preparing a polycrystalline composite material, when heated, after the sodium chloride melts, the small-sized magnesium oxide and zirconium oxide particles can wrap around the molten sodium chloride, which to a certain extent limits the turbulence of the molten sodium chloride, thereby improving the uniformity of the pressure distribution and temperature distribution in the synthesis cavity, thereby reducing the performance of the polycrystalline composite material and the qualified rate of the finished product.
[0009] Preferably, among all the sodium chloride particles, the mass fraction of the sodium chloride particles with a particle size of 100-200 mesh is 50-75%. Further preferably, among all the sodium chloride particles, the mass fraction of the sodium chloride particles with a particle size of 100-200 mesh is 60-75%.
[0010] Preferably, the mass fraction of the magnesium oxide is 1% to 49%. Preferably, the mass fraction of the zirconium oxide is 1% to 48%. If the mass fraction of magnesium oxide and zirconium oxide is too large, the mass of sodium chloride will be too small, which is not conducive to the uniform formation of the temperature field during sintering; if the mass fraction of magnesium oxide and zirconium oxide is too small, the effect of supporting and inhibiting the flow of molten sodium chloride will be weak, and the deformation of the polycrystalline composite material during sintering cannot be effectively reduced.
[0011] Preferably, the insulating material used to synthesize the polycrystalline composite material also includes graphite powder. Preferably, the carbon content of the graphite powder is not less than 99.9%. The graphite powder is used as a molding agent to facilitate the molding of the insulating material to obtain an insulating material (insulating sheet or insulating tube) of a certain shape, so as to be better used for synthesizing the polycrystalline composite material.
[0012] In order to ensure the molding density of the insulating material, and thus ensure that the formed insulating material has good insulation performance and pressure transmission performance, preferably, the particle size of the graphite powder is not less than 200 meshes.
[0013] Preferably, in the insulating material for synthesizing polycrystalline composite materials, the mass fraction of the graphite powder is not greater than 10%. Further preferably, in the insulating material for synthesizing polycrystalline composite materials, the mass fraction of the graphite powder is 3-7%. Too high a mass fraction of graphite powder will affect the insulation of the insulating material.
[0014] The technical solution adopted by the method for preparing the insulating material for synthesizing polycrystalline composite materials of the present invention is:
[0015] A method for preparing the insulating material for synthesizing polycrystalline composite materials as described above comprises the following steps: uniformly mixing the components constituting the insulating material for synthesizing polycrystalline composite materials according to a proportion.
[0016] The method for preparing an insulating material for synthesizing a polycrystalline composite material of the present invention is simple to operate. When the prepared insulating material is used as an insulating sheet for preparing a polycrystalline composite material, the prepared polycrystalline composite material is not prone to deformation, cracking, delamination, carbonization and other problems, and the qualified rate of the product can be effectively improved.
[0017] Preferably, the insulating material for synthesizing polycrystalline composite materials is composed of sodium chloride, magnesium oxide and zirconium oxide. The preparation method of the insulating material for synthesizing polycrystalline composite materials comprises the following steps: uniformly mixing the formulated amounts of sodium chloride, magnesium oxide and zirconium oxide.
[0018] Preferably, the insulating material for synthesizing polycrystalline composite materials further comprises graphite powder. The method for preparing the insulating material for synthesizing polycrystalline composite materials comprises the following steps: uniformly mixing the formulated amounts of sodium chloride, magnesium oxide, zirconium oxide and graphite powder.
[0019] It is understandable that when the insulating material for synthesizing polycrystalline composite materials of the present invention is used to synthesize polycrystalline composite materials, the insulating material can be pressed or sintered after pressing according to the specific application conditions to obtain an insulating material of a specific shape. For example, when the insulating material of the present invention is used as an insulating sheet, the insulating material for synthesizing polycrystalline composite materials of the present invention is pressed and formed by a tablet press to obtain a sheet-like insulating material. When the insulating material of the present invention is used as an insulating tube, the insulating material for synthesizing polycrystalline composite materials of the present invention is first pressed and formed by a hydraulic press to obtain a semi-finished product, and then sintered to obtain a tubular insulating material.
[0020] When the insulating material for synthesizing polycrystalline composite materials of the present invention is used as an insulating sheet or an insulating tube for synthesizing a polycrystalline diamond composite sheet, the temperature used for sintering the polycrystalline diamond composite sheet blank is 1300-1500° C. and the pressure is 5-8 GPa.
[0021] When the insulating material for synthesizing polycrystalline composite materials of the present invention is used as an insulating sheet or an insulating tube to synthesize a cubic boron nitride composite sheet, the temperature used for sintering the cubic boron nitride composite sheet blank is 1300-1500° C. and the pressure is 5-8 GPa. DETAILED DESCRIPTION
[0022] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0023] The carbon content of the graphite powder used in Examples 1-5 and Comparative Examples 1-4 is greater than 99.9%.
[0024] 1. The specific embodiments of the insulating material for synthesizing polycrystalline composite materials of the present invention are as follows:
[0025] Example 1
[0026] The insulating material used to synthesize the polycrystalline composite material of this embodiment is composed of sodium chloride, magnesium oxide, zirconium oxide and graphite powder, wherein the mass fraction of sodium chloride is 65%, the mass fraction of magnesium oxide is 15%, the mass fraction of zirconium oxide is 15%, and the mass fraction of graphite powder is 5%;
[0027] The particle size of sodium chloride is finer than 100 mesh. Among all the sodium chloride particles, the mass fraction of sodium chloride particles with a particle size of 100 mesh to 200 mesh is 60%;
[0028] The particle sizes of magnesium oxide, zirconium oxide and graphite powder are all 200 mesh or finer.
[0029] Example 2
[0030] The insulating material used to synthesize the polycrystalline composite material of this embodiment is composed of sodium chloride, magnesium oxide, zirconium oxide and graphite powder, wherein the mass fraction of sodium chloride is 77%, the mass fraction of magnesium oxide is 10%, the mass fraction of zirconium oxide is 10%, and the mass fraction of graphite powder is 3%;
[0031] The particle size of sodium chloride is finer than 100 mesh, and the mass fraction of sodium chloride particles with a particle size of 100 mesh to 200 mesh is 50% among all sodium chloride particles;
[0032] The particle sizes of magnesium oxide, zirconium oxide and graphite powder are all 200 mesh or finer.
[0033] Example 3
[0034] The insulating material used to synthesize the polycrystalline composite material of this embodiment is composed of sodium chloride, magnesium oxide, zirconium oxide and graphite powder, wherein the mass fraction of sodium chloride is 53%, the mass fraction of magnesium oxide is 20%, the mass fraction of zirconium oxide is 20%, and the mass fraction of graphite powder is 7%;
[0035] The particle size of sodium chloride is finer than 100 mesh. Among all the sodium chloride particles, the mass fraction of sodium chloride particles with a particle size of 100 mesh to 200 mesh is 60%;
[0036] The particle sizes of magnesium oxide, zirconium oxide and graphite powder are all 200 mesh or finer.
[0037] Example 4
[0038] The insulating material for synthesizing the polycrystalline composite material of this embodiment is composed of sodium chloride, magnesium oxide, zirconium oxide and graphite powder, wherein the mass fraction of sodium chloride is 50%, the mass fraction of magnesium oxide is 1%, the mass fraction of zirconium oxide is 48%, and the mass fraction of graphite powder is 1%;
[0039] The particle size of sodium chloride is finer than 100 mesh. Among all the sodium chloride particles, the mass fraction of sodium chloride particles with a particle size of 100 mesh to 200 mesh is 75%;
[0040] The particle sizes of magnesium oxide, zirconium oxide and graphite powder are all 200 mesh or finer.
[0041] Example 5
[0042] The insulating material for synthesizing the polycrystalline composite material of this embodiment is composed of sodium chloride, magnesium oxide, zirconium oxide and graphite powder, wherein the mass fraction of sodium chloride is 50%, the mass fraction of magnesium oxide is 49%, the mass fraction of zirconium oxide is 1%, and the mass fraction of graphite powder is 0%;
[0043] The particle size of sodium chloride is finer than 100 mesh. Among all the sodium chloride particles, the mass fraction of sodium chloride particles with a particle size of 100 mesh to 200 mesh is 75%;
[0044] The particle sizes of magnesium oxide and zirconium oxide are both 200 mesh or finer.
[0045] Comparative Example 1
[0046] The only difference between the insulating material for synthesizing polycrystalline composite materials in this comparative example and the insulating material for synthesizing polycrystalline composite materials in Example 1 is that in the insulating material for synthesizing polycrystalline composite materials in this comparative example, the mass fraction of magnesium oxide is 30%, and the mass fraction of zirconium oxide is 0%.
[0047] Comparative Example 2
[0048] The only difference between the insulating material for synthesizing polycrystalline composite materials in this comparative example and the insulating material for synthesizing polycrystalline composite materials in Example 1 is that in the insulating material for synthesizing polycrystalline composite materials in this comparative example, the mass fraction of magnesium oxide is 0%, and the mass fraction of zirconium oxide is 30%.
[0049] Comparative Example 3
[0050] The only difference between the insulating material for synthesizing polycrystalline composite materials in this comparative example and the insulating material for synthesizing polycrystalline composite materials in Example 1 is that in the insulating material for synthesizing polycrystalline composite materials in this comparative example, the particle size of sodium chloride is 200 mesh or finer.
[0051] Comparative Example 4
[0052] The only difference between the insulating material for synthesizing polycrystalline composite materials in this comparative example and the insulating material for synthesizing polycrystalline composite materials in Example 1 is that in the insulating material for synthesizing polycrystalline composite materials in this comparative example, the particle size of sodium chloride is 50-100 meshes.
[0053] The insulating materials for synthesizing polycrystalline composite materials of Comparative Examples 1-4 are prepared by a method comprising the following steps: the components constituting the insulating materials for synthesizing polycrystalline composite materials are mixed uniformly according to a proportion using a stirring device to obtain the insulating materials.
[0054] 2. The specific embodiment of the method for preparing the insulating material for synthesizing the polycrystalline composite material of the present invention is as follows:
[0055] The preparation method of the insulating material for synthesizing the polycrystalline composite material of Examples 1-5 specifically comprises the following steps:
[0056] The sodium chloride, magnesium oxide, zirconium oxide and graphite powder in the formula amount are mixed evenly by a three-dimensional mixer to obtain an insulating material for synthesizing a polycrystalline composite material.
[0057] Experimental example
[0058] In order to investigate the use effect of insulating materials for synthesizing polycrystalline composite materials with different formulations, sodium chloride, the insulating materials for synthesizing polycrystalline composite materials of Examples 1-5 and Comparative Examples 1-4 were respectively pressed at a pressure of 4MPa using a tablet press to obtain an insulating sheet with a thickness of 2.7mm, and then the density of the insulating sheets made of different insulating materials was tested, and the pressed insulating sheets were placed at the top and bottom of the synthesis cavity as insulating media, and the synthetic blocks for synthesizing polycrystalline diamond composite sheets were assembled, and then the synthetic blocks were placed in a six-sided top press, and then the polycrystalline diamond composite sheet blanks were pressurized and sintered (the pressure sintering temperature was 1400°C and the pressure was 6.0GPa) to obtain polycrystalline diamond composite sheets (polycrystalline diamond composite sheets were all cylindrical, with equal height and diameter of 60mm). Then the wear ratio and impact toughness of the polycrystalline diamond composite sheets made of different insulating sheets were tested. For intuitive comparison, the density of the insulating sheet made of sodium chloride was set to 1, and the ratio of the density of the insulating sheet made of the insulating materials of Examples 1-5 and Comparative Examples 1-4 to the density of the insulating sheet made of sodium chloride was calculated, and the ratio was defined as relative density; at the same time, the wear ratio of the polycrystalline diamond composite sheet prepared by sodium chloride was set to 1, and then the ratio of the wear ratio of the polycrystalline diamond composite sheet prepared by the insulating materials of Examples 1-5 and Comparative Examples 1-4 to the wear ratio of the polycrystalline diamond composite sheet prepared by sodium chloride was calculated, and the calculated ratios were defined as relative wear ratios.
[0059] In order to evaluate the use stability of insulating materials for synthesizing polycrystalline composite materials with different formula compositions, polycrystalline diamond composite sheets were prepared using different insulating sheets according to the above method. The number of samples of polycrystalline diamond composite sheets prepared using the same insulating sheet was 50. Then, the appearance of the two end faces (the two end faces in contact with the insulating sheet) of the polycrystalline diamond composite sheets prepared using different insulating sheets was observed to see if there were cracks, delamination or carbonization. If a sample had cracks, delamination or carbonization, the appearance quality test result of the sample was unqualified. Finally, the appearance quality pass rate of the polycrystalline diamond composite sheets prepared from each insulating sheet was counted. At the same time, the deformation of the polycrystalline diamond composite sheet was tested, and then the average deformation of the polycrystalline diamond composite sheet prepared from each insulating sheet was counted, and the deformation of the polycrystalline diamond composite sheet was evaluated with the calculated average value. The testing method for the deformation of a polycrystalline diamond composite sheet is as follows: first, one bottom surface of the cylindrical composite sheet is brought into contact with a flat reference surface so that the cylindrical composite sheet is placed on the flat reference surface, and then the maximum value of the gap width between the bottom surface in contact with the flat reference surface and the flat reference surface is tested, marked as A, and then the maximum value of the gap width between the other bottom surface of the cylindrical composite sheet and the flat reference surface is tested according to the above method, marked as B, then the deformation of the polycrystalline diamond composite sheet is the maximum value of A and B.
[0060] The relative density of the insulating sheets made of different insulating materials, the relative wear ratio and average deformation value of the polycrystalline diamond composite sheets made of different insulating materials, and the appearance quality pass rate are shown in Table 1.
[0061] Table 1 Relative density of insulating sheets made of different insulating materials, relative wear ratio and average deformation of polycrystalline diamond composite sheets made of different insulating materials, and appearance quality pass rate
[0062]
[0063]
[0064] In addition, after sodium chloride, the insulating materials for synthesizing polycrystalline composite materials of Examples 1-5 and Comparative Examples 1-4 were respectively pressed by a tablet press to obtain insulating sheets, and then the insulating sheets were used to synthesize polycrystalline cubic boron nitride composite sheets. Experimental results showed that, compared with the polycrystalline cubic boron nitride composite sheets prepared by using sodium chloride and the insulating materials for synthesizing polycrystalline composite materials of Comparative Examples 1-4 as insulating sheets, the polycrystalline cubic boron nitride composite sheets prepared by using the insulating materials for synthesizing polycrystalline composite materials of Examples 1-5 had significantly reduced cracks, delamination or carbonization, and the deformation was also reduced, while the wear ratio was improved.
Claims
1. An insulating material for synthesizing polycrystalline composite materials, characterized in that: The invention is composed of sodium chloride, magnesium oxide, graphite powder and zirconium oxide, wherein sodium chloride particles with larger particle size are selected to be used in combination with magnesium oxide and zirconium oxide particles with smaller particle sizes, the mass fraction of the sodium chloride is not less than 50%, the mass fraction of the magnesium oxide is not less than 1%, the mass fraction of the zirconium oxide is not less than 1%, the particle size of the sodium chloride is not less than 100 mesh, the particle size of the magnesium oxide is not less than 200 mesh, and the particle size of the zirconium oxide is not less than 200 mesh; among all the sodium chloride particles, the mass fraction of the sodium chloride particles with a particle size of 100 mesh to 200 mesh is 50 to 75%; the particle size of the graphite powder is not less than 200 mesh, and the mass fraction is not more than 10%.
2. The insulating material for synthesizing polycrystalline composite materials according to claim 1, characterized in that: Among all the sodium chloride particles, the mass fraction of the sodium chloride particles with a particle size of 100 mesh to 200 mesh is 60~75%.
3. The insulating material for synthesizing polycrystalline composite materials according to claim 1, characterized in that: The mass fraction of the magnesium oxide is 1% to 49%.
4. The insulating material for synthesizing polycrystalline composite materials according to claim 1, characterized in that: The mass fraction of the zirconium oxide is 1% to 48%.
5. A method for preparing an insulating material for synthesizing a polycrystalline composite material according to any one of claims 1 to 4, characterized in that: The following steps are involved: The components constituting the insulating material for synthesizing the polycrystalline composite material are mixed uniformly according to a proportion.