A high temperature resistant, long life, ablation resistant ceramic modified carbon / carbon composite material and its preparation method and application

By combining thermal gradient chemical vapor deposition method and vacuum infiltration method, HfC-ZrC-Cu synergistically modified C/C composite material was prepared, which solved the problem of C/C composite material being easily oxidized in high-temperature aerobic environment and achieved The densification and oxidation resistance of the material are improved, which significantly improves the resistance to cyclic ablation.

CN116803953BActive Publication Date: 2024-10-01WUXI BOZHI COMPOSITE MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310795454.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-30
Publication Date
2024-10-01
Estimated Expiration
2043-06-30

AI Technical Summary

Technical Problem

Existing C/C composite materials are prone to oxidation in high-temperature aerobic environments, resulting in poor ablation resistance, and damage to fibers by the melt during the preparation process results in poor material performance.

Method used

The thermal gradient chemical vapor deposition method is combined with the vacuum impregnation method, and the HfC ceramic precursor is uniformly mixed with xylene, followed by multiple impregnation and ultrasonic vibration treatments, followed by high-temperature heat treatment under argon protection, and finally Zr- Cu powder is embedded to achieve densification and improved oxidation resistance of the material.

Benefits of technology

HfC-ZrC-Cu synergistically modified C/C composite materials with high density and excellent cyclic ablation resistance were prepared, which can maintain integrity at high temperatures for a long time, and the mass ablation rate and line ablation rate are significantly reduced, showing excellent performance Excellent high temperature resistance, long life and ablation resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116803953B_ABST
    Figure CN116803953B_ABST
Patent Text Reader

Abstract

The present invention discloses a high temperature resistant, long life, ablation resistant ceramic modified carbon / carbon composite material and its preparation method and application, belonging to the technical field of preparation of oxidation resistant and ablation resistant carbon / carbon composite materials. The present invention introduces HfC ultra-high temperature ceramics into a porous C / C composite material through PIP to achieve uniform distribution of HfC ultra-high temperature ceramics in a carbon matrix. By reacting Zr‑Cu powder with a carbon matrix to generate ZrC, rapid densification of the matrix at low temperature is achieved, and a ceramic modified C / C composite material that can be used for a long time in a high flow and strong erosion and ablation environment is prepared. The HfC‑ZrC‑Cu synergistically modified C / C composite material prepared by the present invention has a heat flux density of 4.18MW / m 2 After 600s of cyclic ablation under oxyacetylene flame, the sample was still intact, and the mass ablation rate and line ablation rate were 0.544mg / s and 0.107μm / s, respectively, showing excellent anti-cyclic ablation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of oxidation-resistant and ablation-resistant carbon / carbon composite materials, and specifically relates to a high-temperature-resistant, long-life ablation-resistant ceramic-modified carbon / carbon composite material and a preparation method and application thereof. Background Art

[0002] Typical working environment characteristics such as "high temperature, long time, oxygen, complex heat / force loads" have put forward urgent demands and severe challenges for thermal protection and thermal structural materials for hypersonic vehicles. It is urgent to develop new high-temperature resistant, long-life anti-oxidation and anti-ablation composite materials to meet the development needs of the aerospace industry and national defense science and technology. C / C composite materials are considered to be one of the most promising new materials due to their low density, high specific strength, high specific modulus, low thermal expansion coefficient, and especially their ability to maintain high strength at ultra-high temperatures. However, their easy oxidation in high-temperature aerobic environments has severely limited their applications.

[0003] Some studies have proposed that ultra-high temperature ceramics can be introduced into the matrix of C / C composites to improve their oxidation resistance, reduce the ablation rate, and enable them to withstand higher gas temperatures or longer working hours. Methods developed by domestic and foreign scholars such as precursor infiltration pyrolysis (PIP), reactive melt infiltration (RMI, chemical vapor infiltration (CVI), gas phase siliconization (GSI), and slurry infiltration (SI) have successfully introduced a variety of antioxidant and ablation ceramics into C / C composites.

[0004] Among them, GSI can produce uniform and dense C / C-SiC composite materials, effectively hinder the penetration of oxygen, and the thermal expansion coefficient is more matched with that of C / C composite materials, and it is not easy to crack at high temperatures. However, it is easy to leave residual Si in the matrix during the gas phase siliconization process. Due to its low melting point and vapor pressure, it evaporates quickly under high temperature environment, which is not conducive to the stability of service performance. The SI process is simple and low in cost, but the particles are easy to agglomerate on the surface of the material, resulting in surface sealing and leaving more pores inside; PIP can introduce multiple ceramics into the C / C composite material at the same time, but the yield of precursor ceramics is low, and it takes multiple impregnation-drying-cracking cycles to prepare dense modified C / C composite materials, resulting in a long production cycle, and the volume shrinkage of the precursor after cracking is large, which is easy to produce cracks and pores; the CVI method can be prepared at a lower temperature, the residual stress inside the material is small, the carbon fiber is almost undamaged, and the composition design on a micro scale can be realized. However, it has high requirements for equipment, long preparation cycle, high production cost, and is prone to form surface "crusting" phenomenon during the preparation process, which affects further densification; RMI has the advantages of short cycle, low cost, low residual porosity and near net forming, but due to the high reaction temperature in the RMI method, there is an inevitable violent reaction between the fiber and the melt, which is easy to cause certain damage to the carbon fiber in the C / C matrix, resulting in poor mechanical properties of the composite material. Therefore, if the RMI method can be organically combined with other preparation processes to avoid damage to the fiber by the melt during the infiltration preparation process, the performance of the composite material can be effectively improved. Summary of the invention

[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a high-temperature resistant, long-life, ablation-resistant ceramic-modified carbon / carbon composite material and its preparation method and application, which can effectively avoid the damage of the melt to the fiber during the preparation process, thereby causing the technical problem of poor anti-cyclic ablation performance of the carbon / carbon composite material.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention discloses a method for preparing a high temperature resistant, long life, ablation resistant ceramic modified carbon / carbon composite material, comprising the following steps:

[0008] 1) uniformly mixing a hafnium carbide (HfC) ceramic precursor with xylene to prepare a HfC ceramic precursor solution;

[0009] 2) Thermal gradient chemical vapor deposition method was used to prepare a density of 1.0-1.3g / cm 3 The C / C composite material is dried for use;

[0010] 3) placing the C / C composite material obtained in step 2) in a HfC ceramic precursor solution for vacuum infiltration treatment, and then drying;

[0011] 4) subjecting the C / C composite material treated in step 3) to ultrasonic vibration treatment and drying for later use;

[0012] 5) subjecting the C / C composite material obtained in step 4) to high temperature heat treatment under an argon protective atmosphere;

[0013] 6) Repeat steps 3) to 5) until the density of the sample increases to 1.5-1.8 g / cm 3 ;

[0014] 7) The sample obtained in step 6) is fully embedded with Zr-Cu powder, and then heated to 1100-1300°C from room temperature under vacuum conditions, kept warm for 2-4 hours, cooled to 800°C, and then cooled to room temperature to obtain a high temperature resistant, long life, ablation resistant ceramic modified carbon / carbon composite material.

[0015] Preferably, in step 1), xylene and HfC ceramic precursor are mixed because HfC ceramic precursor has good dispersibility in xylene.

[0016] Preferably, in step 1), in the HfC ceramic precursor solution, the HfC ceramic precursor accounts for 40% to 50% of the total mass of the HfC ceramic precursor solution, and the xylene accounts for 50% to 60%.

[0017] Preferably, in step 2), the specific operations include:

[0018] The 2.5D needle-punched carbon felt preform was deposited at a pressure of 6-12 kPa and a temperature of 900-1200 °C for 15-25 h, and the flow rate of natural gas during the deposition process was controlled at 2-5 L / min. After the deposition was completed, it was cooled to room temperature to obtain a density of 1.0-1.3 g / cm 3 C / C composite materials.

[0019] Further preferably, in step 2), the obtained density is 1.0-1.3 g / cm 3 The C / C composite material is processed into a disc sample for ablation test. The reason for processing into a disc sample is to facilitate ablation test.

[0020] In step 2), the C / C composite material is ultrasonically cleaned in anhydrous ethanol for 10-30 minutes and then placed in an oven at 60-90° C. to dry for 1-3 hours for later use.

[0021] Preferably, in step 3), a 3The C / C composite material is placed in the HfC ceramic precursor solution obtained in step 1), and vacuum impregnation treatment is performed under a vacuum degree of 0.05-0.1 MPa for 30-60 min, and then the C / C composite material is taken out and dried at 60-100° C. for 24-48 h. The vacuum impregnation treatment is to make it easier for the HfC ceramic precursor to infiltrate into the interior of the C / C composite material.

[0022] Preferably, in step 4), the C / C composite material treated in step 3) is placed in xylene, ultrasonically vibrated for 1-3 minutes at an ultrasonic power of 50-100 W, and then taken out and dried at 60-90° C. for 1-3 hours for later use. This step will remove the precursors that are not firmly bonded.

[0023] In step 5), the C / C composite material treated in step 4) is treated at 1600-1850° C. for 1-2 h under argon protection.

[0024] Preferably, in step 7), the vacuum is evacuated to 1.0×10 -2 MPa; heating to 1100-1300°C at a heating rate of 5°C / min; cooling to 800°C at a cooling rate of 5°C / min, and cooling to room temperature along with the furnace to obtain a high-temperature resistant, long-life, ablation-resistant ceramic modified carbon / carbon composite material, namely, a dense HfC-ZrC-Cu modified C / C composite material.

[0025] The invention also discloses a high temperature resistant, long life, ablation resistant ceramic modified carbon / carbon composite material prepared by the above preparation method.

[0026] The present invention also discloses the application of the above-mentioned high temperature resistant, long life, ablation resistant ceramic modified carbon / carbon composite material in the preparation of hypersonic aircraft.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The preparation method of the high temperature resistant, long life and ablation resistant ceramic modified carbon / carbon composite material disclosed in the present invention proposes for the first time an innovative idea of ​​preparing HfC-ZrC-Cu synergistic modified C / C composite material by combining the PIP process and the low temperature RMI process. On the one hand, HfC ultra-high temperature ceramics are introduced into the porous C / C composite material by PIP to achieve uniform distribution of HfC ultra-high temperature ceramics in the carbon matrix. On the other hand, the low temperature RMI process is adopted to generate ZrC by the reaction of Zr-Cu powder with the carbon matrix to achieve rapid densification of the matrix at low temperature, and prepare a ceramic modified C / C composite material that can be used for a long time in a large flow and strong erosion and ablation environment. The low temperature RMI process not only reduces the damage to the fiber during the reaction infiltration process, but also slows down the Zr-C reaction rate, thereby improving the density of the material.

[0029] The experimental results show that the HfC-ZrC-Cu synergistic modified C / C composite material prepared by the present invention has a heat flux density of 4.18MW / m 2 After 600s of cyclic ablation under oxyacetylene flame, the sample was still intact, and the mass ablation rate and line ablation rate were 0.544mg / s and 0.107μm / s, respectively, showing excellent anti-cyclic ablation performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 XRD pattern of HfC-ZrC-Cu synergistically modified C / C composite material;

[0031] Figure 2 SEM images and EDS spectra of HfC-ZrC-Cu synergistically modified C / C composites; (a) is a high-magnification image; (b) and (c) are low-magnification images; (d), (e) and (f) are EDS spectra;

[0032] Figure 3 The macroscopic morphology photos of HfC-ZrC-Cu synergistically modified C / C composites before and after ablation: (a) before ablation; (b) after ablation for 120s; (c) after ablation for 240s; (d) after ablation for 360s; (e) after ablation for 480s; (f) after ablation for 600s;

[0033] Figure 4 Microscopic morphology photos and EDS spectra of the center and edge areas of the HfC-ZrC-Cu synergistically modified C / C composite material after 600s cyclic ablation: (a) and (b) are the center area; (c) EDS spectrum;

[0034] Figure 5 Cross-sectional SEM images and EDS spectra of HfC-ZrC-Cu synergistically modified C / C composites after 600s cyclic ablation: (a) low-magnification image; (b) high-magnification image; (c), (d), (e) and (f) are the surface energy spectra of C, O, Zr and Hf elements, respectively. DETAILED DESCRIPTION

[0035] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0036] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0037] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0038] The hafnium carbide ceramic precursor (HfC ceramic precursor) used in the following embodiments of the present invention was purchased from the Institute of Process Engineering, Chinese Academy of Sciences.

[0039] Example 1

[0040] 1) Weighing a certain proportion of HfC ceramic precursor and xylene, wherein the mass fraction of the organic hafnium polymer is 40wt% and the mass fraction of xylene is 60wt%, and then ultrasonically treating and magnetically stirring to obtain a HfC ceramic precursor solution;

[0041] 2) The 2.5D needle-punched carbon felt preform was cleaned and dried and placed in a thermal gradient furnace. The pressure in the deposition furnace was then pumped down to 8 kPa using a vacuum pump. Deposition was performed at 1000°C for 20 hours. The flow rate of natural gas during the deposition process was controlled to be 3.5 L / min. After the deposition was completed, the power was turned off and the temperature was cooled to room temperature to obtain a low-density C / C composite material.

[0042] 3) The density of the film prepared by thermal gradient chemical vapor deposition is 1.0 g / cm 3 The low-density C / C was processed into a disc with a size of Φ30mm×5mm, ultrasonically cleaned in anhydrous ethanol for 10 minutes, and then placed in an oven to dry at 60℃ for 3 hours for use;

[0043] 4) The sample obtained in step 3) was placed in the HfC ceramic precursor solution obtained in step 1) for infiltration, and the vacuum degree was controlled to be 0.1 MPa for infiltration for 30 minutes. The sample was then taken out and dried in an oven at 70° C. for 40 hours;

[0044] 5) placing the sample obtained in step 4) in xylene for ultrasonic oscillation for 1 min at an ultrasonic power of 100 W, taking it out and drying it in an oven at 90° C. for 1 h before use;

[0045] 6) placing the sample obtained in step 5) into a high temperature heat treatment furnace and treating it at 1650° C. for 1.5 h under argon protection;

[0046] 7) Repeat steps 4) to 6) until the sample density increases to 1.5-1.8 g / cm 3 ;

[0047] 8) A layer of Zr-Cu powder with a thickness of 8 mm was spread on the bottom of the graphite crucible, and the sample obtained in step 7) was placed on the Zr-Cu powder. Then, Zr-Cu powder was added to fully bury the sample. After the graphite crucible was sealed, it was placed in a vacuum hot press furnace and vacuumed to 1.0×10 -2 MPa; heat to 1100°C at a heating rate of 5°C / min, keep warm for 4h, cool to 800°C at a cooling rate of 5°C / min; then turn off the power and cool with the furnace to prepare HfC-ZrC-Cu modified C / C composite material.

[0048] See also Figure 1 , is the XRD pattern of HfC-ZrC-Cu synergistically modified C / C composite material. Figure 1 It can be seen that HfC, ZrC, Cu and C were detected on the surface of the prepared ultra-high temperature ceramic modified sample. Since the diffraction angles of the characteristic peaks of HfC and ZrC are close, their peaks in the XRD diagram overlap. Among them, HfC is introduced into the C / C composite material by the PIP process, and ZrC and Cu are generated by the reaction of Zr-Cu alloy powder and carbon matrix, indicating that PIP combined with low-temperature RMI process can successfully realize the co-modification of C / C composite materials by multi-ceramics.

[0049] Example 2

[0050] 1) Weighing a certain proportion of HfC ceramic precursor and xylene, wherein the mass fraction of the organic hafnium polymer is 45wt% and the mass fraction of the xylene is 55wt%, and then ultrasonically treating and magnetically stirring to obtain a HfC ceramic precursor solution;

[0051] 2) After cleaning and drying the 2.5D needle-punched carbon felt preform, put it into a thermal gradient furnace, and then use a vacuum pump to pump the pressure in the deposition furnace to 10 kPa, and deposit it at 950°C for 20 hours. During the deposition process, the flow rate of natural gas is controlled to 4 L / min. After the deposition is completed, the power is turned off and the temperature is cooled to room temperature to obtain a low-density C / C composite material;

[0052] 3) The density of the film prepared by thermal gradient chemical vapor deposition is 1.15 g / cm 3 The low-density C / C was processed into a disc with a size of Φ30mm×5mm, ultrasonically cleaned in anhydrous ethanol for 15min, and then placed in an oven to dry at 70℃ for 2.5h for use;

[0053] 4) The sample obtained in step 3) was placed in the HfC ceramic precursor solution obtained in step 1) for infiltration, and the vacuum degree was controlled to be 0.08 MPa for infiltration for 45 minutes. The sample was then taken out and dried in an oven at 60° C. for 48 hours;

[0054] 5) placing the sample obtained in step 4) in xylene and subjecting it to ultrasonic vibration for 3 min at an ultrasonic power of 50 W, taking it out and placing it in an oven to dry at 90° C. for 1 h before use;

[0055] 6) placing the sample obtained in step 5) into a high temperature heat treatment furnace and treating it at 1600° C. for 2 h under argon protection;

[0056] 7) Repeat steps 4) to 6) until the sample density increases to 1.5-1.8 g / cm 3 ;

[0057] 8) A layer of Zr-Cu powder with a thickness of 12 mm was spread on the bottom of the graphite crucible, and the sample obtained in step 7) was placed on the Zr-Cu powder, and then Zr-Cu powder was added to fully bury the sample. After the graphite crucible was sealed, it was placed in a vacuum hot press furnace and vacuumed to 1.0×10 -2 MPa; heat to 1250°C at a heating rate of 5°C / min, keep warm for 2h, cool to 800°C at a cooling rate of 5°C / min; then turn off the power and cool with the furnace to prepare HfC-ZrC-Cu modified C / C composite material.

[0058] See also Figure 2 As can be seen from the figure, after the PIP combined with low-temperature RMI process, a large number of HfC particles and Zr melt infiltrated into the C / C composite material, and the carbides were evenly distributed in the matrix. The cross section of the composite material is composed of black, gray, and white phases as well as the dispersed structure inside. There are very few holes in the composite material, but no obvious cracks. According to the EDS spectrum ( Figure 2 From the analysis of (d), (e), and (f), we can see that the black phase particles are mainly composed of C, the gray phase particles are mainly composed of Zr, C, and Cu, and the white phase particles are mainly composed of Hf, C, and Cu. Combined with XRD analysis, we can see that the black phase is C, the gray phase is ZrC, the white phase is HfC, and the substance dispersed in the gray-white phase is residual metal Cu ( Figure 2 (c)).

[0059] Example 3

[0060] 1) Weighing a certain proportion of HfC ceramic precursor and xylene, wherein the mass fraction of the organic hafnium polymer is 50wt%, and the mass fraction of the xylene is 50wt%, and then ultrasonically treating and magnetically stirring to obtain a HfC ceramic precursor solution;

[0061] 2) After cleaning and drying the 2.5D needle-punched carbon felt preform, the preform was placed in a thermal gradient furnace, and then the pressure in the deposition furnace was pumped down to 12 kPa by a vacuum pump, and deposition was performed at 900°C for 25 hours. During the deposition process, the flow rate of natural gas was controlled to be 5 L / min. After the deposition was completed, the power was turned off and the temperature was cooled to room temperature to obtain a low-density C / C composite material;

[0062] 3) The density of the film prepared by thermal gradient chemical vapor deposition is 1.2 g / cm 3 The low-density C / C was processed into a disc with a size of Φ30mm×5mm, ultrasonically cleaned in anhydrous ethanol for 20min, and then dried in an oven at 80℃ for 1.5h for use;

[0063] 4) The sample obtained in step 3) was placed in the HfC ceramic precursor solution obtained in step 1) for infiltration, and the vacuum degree was controlled to be 0.05 MPa for infiltration for 60 minutes. The sample was then taken out and dried in an oven at 80° C. for 36 hours;

[0064] 5) placing the sample obtained in step 4) in xylene and subjecting it to ultrasonic vibration for 2 min at an ultrasonic power of 80 W, taking it out and placing it in an oven to dry at 60° C. for 3 h before use;

[0065] 6) placing the sample obtained in step 5) into a high temperature heat treatment furnace and treating it at 1850° C. for 1 h under argon protection;

[0066] 7) Repeat steps 4) to 6) until the sample density increases to 1.5-1.8 g / cm 3 ;

[0067] 8) A layer of Zr-Cu powder with a thickness of 10 mm was spread on the bottom of the graphite crucible, and the sample obtained in step 7) was placed on the Zr-Cu powder. Then, Zr-Cu powder was added to fully bury the sample. After the graphite crucible was sealed, it was placed in a vacuum hot press furnace and vacuumed to 1.0×10 -2 MPa; heat to 1200°C at a heating rate of 5°C / min, keep warm for 3h, then cool to 800°C at a cooling rate of 5°C / min; then turn off the power and cool with the furnace to prepare the HfC-ZrC-Cu modified C / C composite material.

[0068] See also Figure 3 , Figure 3 The macroscopic morphology of the HfC-ZrC-Cu synergistically modified C / C composite material prepared in this embodiment before and after ablation. Figure 3 It can be seen that a layer of white solid covering appears on the surface of the samples after ablation. Figure 3It can be seen in (b) and (c) that after ablation for 120s and 240s, the white area on the surface of the HfC-ZrC-Cu synergistically modified C / C composite material is basically intact, and there is no exposure of the black carbon matrix. Figure 3 As shown in (d), the white area in the ablation center of the HfC-ZrC-Cu synergistically modified C / C composite material becomes incomplete. Figure 3 After 600s ablation, the oxide film on the surface of the HfC-ZrC-Cu synergistically modified C / C composite material has no obvious changes ( Figure 3 As shown in (f), the oxide film in the central area almost covers the internal material in the entire area, indicating that the composite material has excellent high temperature resistance, long life and anti-ablation performance.

[0069] Example 4

[0070] 1) Weighing a certain proportion of HfC ceramic precursor and xylene, wherein the mass fraction of the organic hafnium polymer is 42wt% and the mass fraction of the xylene is 58wt%, and then ultrasonically treating and magnetically stirring to obtain a HfC ceramic precursor solution;

[0071] 2) After cleaning and drying the 2.5D needle-punched carbon felt preform, the preform was placed in a thermal gradient furnace, and then the pressure in the deposition furnace was pumped down to 6 kPa by a vacuum pump, and the deposition was performed at 1200°C for 15 hours. During the deposition process, the flow rate of natural gas was controlled to be 2 L / min. After the deposition was completed, the power was turned off and the temperature was cooled to room temperature to obtain a low-density C / C composite material;

[0072] 3) The density of the film prepared by thermal gradient chemical vapor deposition is 1.25 g / cm 3 The low-density C / C was processed into a disc with a size of Φ30mm×5mm, ultrasonically cleaned in anhydrous ethanol for 25min, and then dried in an oven at 80℃ for 2h for use;

[0073] 4) The sample obtained in step 3) was placed in the HfC ceramic precursor solution obtained in step 1) for infiltration, and the vacuum degree was controlled to be 0.06MPa for infiltration for 50min. The sample was then taken out and dried in an oven at 90°C for 30h;

[0074] 5) placing the sample obtained in step 4) in xylene and subjecting it to ultrasonic vibration for 2 minutes at an ultrasonic power of 70W, taking it out and placing it in an oven to dry at 80°C for 1.5 hours for later use;

[0075] 6) placing the sample obtained in step 5) into a high temperature heat treatment furnace and treating it at 1700° C. for 1.5 h under argon protection;

[0076] 7) Repeat steps 4) to 6) until the sample density increases to 1.5-1.8 g / cm 3 ;

[0077] 8) A layer of Zr-Cu powder with a thickness of 15 mm was spread on the bottom of the graphite crucible, and the sample obtained in step 7) was placed on the Zr-Cu powder, and then Zr-Cu powder was added to fully bury the sample. After the graphite crucible was sealed, it was placed in a vacuum hot press furnace and vacuumed to 1.0×10 -2 MPa; heat to 1300°C at a heating rate of 5°C / min, keep warm for 2h, cool to 800°C at a cooling rate of 5°C / min; then turn off the power and cool with the furnace to prepare HfC-ZrC-Cu modified C / C composite material.

[0078] Figure 4 The SEM photos and EDS spectra of the center and edge regions of the HfC-ZrC-Cu synergistic modified C / C composite material prepared in this example after cyclic ablation. Figure 4 (a) It can be seen that when the heat flux is 4.18 MW / m 2 After 600s of cycling in the oxyacetylene ablation environment, a dense oxide layer formed on the surface of the sample. Figure 4 (a) It can be seen that the sample is still intact after cyclic ablation, and no obvious oxidation ablation phenomenon occurs. Figure 4 (c) Analysis shows that this area is mainly composed of Zr, Hf and O elements. The central area of ​​the ablated sample ( Figure 4 The glassy material generated in (a) is ZrO 2 and HfO 2 The solid solution is formed by high-temperature melting. Under the action of strong airflow, the melt spreads on the surface of the ablated sample to form a barrier layer, preventing the oxidizing atmosphere from entering the interior of the material, which plays a key role in improving the material's anti-ablation performance. Figure 4 It can also be seen in (b) that there are some micropores on the central surface. 2 The large amount of gas released to the outside of the material will cause the surface HfO to be ablated. 2 -ZrO 2 The protective layer forms holes. The volatilization of Cu will have a sweating effect, reducing the ablation temperature of the sample surface, thereby improving the long-term anti-ablation performance of the sample.

[0079] Example 5

[0080] 1) Weighing a certain proportion of HfC ceramic precursor and xylene, wherein the mass fraction of the organic hafnium polymer is 48wt% and the mass fraction of the xylene is 52wt%, and then ultrasonically treating and magnetically stirring to obtain a HfC ceramic precursor solution;

[0081] 2) After cleaning and drying the 2.5D needle-punched carbon felt preform, the preform was placed in a thermal gradient furnace, and then the pressure in the deposition furnace was pumped down to 9 kPa by a vacuum pump, and the deposition was performed at 1100° C. for 18 h. During the deposition process, the flow rate of natural gas was controlled to be 3 L / min. After the deposition was completed, the power was turned off and the temperature was cooled to room temperature to obtain a low-density C / C composite material;

[0082] 3) The density of the film prepared by thermal gradient chemical vapor deposition is 1.3 g / cm 3 The low-density C / C was processed into a disc with a size of Φ30mm×5mm, ultrasonically cleaned in anhydrous ethanol for 30min, and then dried in an oven at 90℃ for 1h for use;

[0083] 4) The sample obtained in step 3) was placed in the HfC ceramic precursor solution obtained in step 1) for infiltration, and the vacuum degree was controlled to be 0.09 MPa for infiltration for 40 minutes. The sample was then taken out and dried in an oven at 100° C. for 24 hours;

[0084] 5) placing the sample obtained in step 4) in xylene and subjecting it to ultrasonic vibration for 1 min at an ultrasonic power of 90 W, taking it out and placing it in an oven to dry at 70° C. for 2 h before use;

[0085] 6) placing the sample obtained in step 5) into a high temperature heat treatment furnace and treating it at 1800° C. for 1 h under argon protection;

[0086] 7) Repeat steps 4) to 6) until the sample density increases to 1.5-1.8 g / cm 3 ;

[0087] 8) A layer of Zr-Cu powder with a thickness of 9 mm was spread on the bottom of the graphite crucible, and the sample obtained in step 7) was placed on the Zr-Cu powder. Then, Zr-Cu powder was added to fully bury the sample. After the graphite crucible was sealed, it was placed in a vacuum hot press furnace and vacuumed to 1.0×10 -2 MPa; heat to 1150°C at a heating rate of 5°C / min, keep warm for 4h, cool to 800°C at a cooling rate of 5°C / min; then turn off the power and cool in the furnace to prepare HfC-ZrC-Cu modified C / C composite material.

[0088] See also Figure 5 , are the cross-sectional SEM photos and EDS spectra of the central area of ​​the HfC-ZrC-Cu synergistic modified C / C composite material obtained in this embodiment after cyclic ablation. Figure 5 It can be seen from (a) and (b) that when the heat flux is 4.18 MW / m 2 After 600s of cyclic ablation in an oxyacetylene ablation environment, there is no ablation dent on the cross section of the sample, and the oxide layer is dense and intact. Figure 5 In (c), (d), (e) and (f), it can be seen that the oxide layer contains a large amount of Zr and Hf elements, indicating that HfO 2 With ZrO 2 The solid solution effect is good. The complete and dense oxide layer is conducive to preventing the further erosion of the internal matrix by the oxyacetylene flame, thereby showing excellent anti-ablation performance.

[0089] In addition, the ablation performance of the HfC-ZrC-Cu synergistically modified C / C composites prepared in Examples 1 to 5 of the present invention was tested, and it was found that the composites had a heat flux density of 4.18 MW / m 2 The sample was still intact after 600s of cyclic ablation under oxyacetylene flame. The comprehensive average data showed that the mass ablation rate and line ablation rate were 0.544mg / s and 0.107μm / s, respectively, showing excellent anti-cyclic ablation performance. The mass ablation rate and line ablation rate of each specific embodiment are shown in Table 1:

[0090] Table 1 Ablation properties of materials prepared in different embodiments

[0091]

[0092] In summary, the present invention adopts PIP combined with low-temperature RMI process to prepare a HfC-ZrC-Cu synergistic modified C / C composite material. On the one hand, the PIP process introduces HfC into the porous C / C composite material to achieve uniform distribution of HfC ceramics in the carbon matrix. On the other hand, the low-temperature reaction infiltration Zr-Cu alloy is used to achieve rapid densification of the C / C-HfC composite material obtained by PIP. The low-temperature RMI process not only reduces the damage to the fiber during the reaction infiltration process, but also slows down the Zr-C reaction rate, thereby improving the density of the material.

[0093] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing a high temperature resistant, long life, ablation resistant ceramic modified carbon / carbon composite material, characterized in that: The following steps are involved: 1) uniformly mixing a hafnium carbide ceramic precursor and xylene to prepare a hafnium carbide ceramic precursor solution; 2) Thermal gradient chemical vapor deposition was used to prepare the nanostructured carbon nanotubes with a density of 1.0-1.3 g / cm 3 The C / C composite material is dried for use; the specific operation includes: depositing the 2.5 D needle-punched carbon felt preform under the conditions of pressure of 6-12 kPa and temperature of 900-1200 °C for 15-25 h, and controlling the flow rate of natural gas during the deposition process to 2-5 L / min, cooling to room temperature after the deposition is completed, and obtaining a density of 1.0-1.3 g / cm 3 C / C composite materials; 3) placing the C / C composite material in a hafnium carbide ceramic precursor solution for vacuum infiltration treatment, and then drying; 4) subjecting the C / C composite material treated in step 3) to ultrasonic vibration treatment and drying for later use; 5) subjecting the C / C composite material obtained in step 4) to high temperature heat treatment under an argon protective atmosphere; 6) Repeat steps 3) to 5) until the density of the C / C composite material increases to 1.5-1.8 g / cm 3 ; 7) Increase the density to 1.5~1.8 g / cm 3 The C / C composite material was fully embedded with Zr-Cu powder and then vacuumed to 1.0×10 -2 MPa, heated from room temperature to 1100-1300°C at a heating rate of 5°C / min, kept warm for 2-4h, cooled to 800°C at a cooling rate of 5°C / min, and then cooled to room temperature with the furnace to obtain a high-temperature resistant, long-life, ablation-resistant ceramic modified carbon / carbon composite material, i.e., a dense HfC-ZrC-Cu modified C / C composite material.

2. The method for preparing the high temperature resistant, long life, ablation resistant ceramic modified carbon / carbon composite material according to claim 1, characterized in that: In step 1), in the hafnium carbide ceramic precursor, the hafnium carbide ceramic precursor accounts for 40% to 50% of the total mass of the hafnium carbide ceramic precursor solution, and xylene accounts for 50% to 60%.

3. The method for preparing the high temperature resistant, long life, ablation resistant ceramic modified carbon / carbon composite material according to claim 1, characterized in that: In step 2), the density of the obtained 3 The C / C composite material was ultrasonically cleaned in anhydrous ethanol for 10-30 min and then dried in an oven at 60-90 °C for 1-3 h for use.

4. The method for preparing the high temperature resistant, long life, ablation resistant ceramic modified carbon / carbon composite material according to claim 1, characterized in that: In step 3), the C / C composite material is placed in the HfC ceramic precursor solution and infiltrated under a vacuum degree of 0.05-0.1 MPa for 30-60 min. The disc sample is then taken out and dried at 60-100 °C for 24-48 h.

5. The method for preparing the high temperature resistant, long life, ablation resistant ceramic modified carbon / carbon composite material according to claim 1, characterized in that: In step 4), the C / C composite material treated in step 3) is placed in xylene and ultrasonically vibrated for 1 to 3 min at an ultrasonic power of 50 to 100 W. After being taken out, it is dried at 60 to 90 ° C for 1 to 3 h and then used for later use.

6. The method for preparing the high temperature resistant, long life, ablation resistant ceramic modified carbon / carbon composite material according to claim 1, characterized in that: In step 5), the reaction mixture is treated at 1600-1850 °C for 1-2 h under argon protection.

7. A high temperature resistant, long life, ablation resistant ceramic modified carbon / carbon composite material prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the high temperature resistant, long life, ablation resistant ceramic modified carbon / carbon composite material according to claim 7 in the preparation of hypersonic aircraft.