A method for preparing hard carbon negative electrode material
By dissolving asphalt and sodium hydroxide at high temperature and mixing them with organic phosphate to form a closed-cell structure, the complex process and high cost in the preparation of hard carbon negative electrode materials are solved, and efficient Coulomb efficiency and capacity improvement are achieved.
Patent Information
- Application Number
- CN202310691454.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-06-11
AI Technical Summary
The existing hard carbon negative electrode material preparation methods are difficult to improve the first effect and platform capacity contribution through closed-cell construction and surface modification, and the process is complex and costly.
After heating and dissolving in a sealed container, it is calcined and crushed in a sealed container, and then mixed with organic phosphate and organic solvent. By spray drying and secondary calcining, a large number of closed-cell structures are formed to improve the efficiency and magnification of Coulomb. performance.
The high capacity, excellent Coulomb efficiency and cycling performance of hard carbon anode materials are achieved, while reducing production costs.
Smart Images

Figure CN116873897B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium ion batteries and relates to a method for preparing a hard carbon negative electrode material. Background Art
[0002] The development and use of clean energy has become a national strategy, and electrochemical energy storage is one of the key technologies. In order to cope with the shortage of lithium resources and the continuous rise in prices, it is urgent to develop new energy storage battery technologies. Sodium-ion batteries have shown great potential in the fields of energy storage and low-speed electric vehicles with their resource and cost advantages, but they still face technical deficiencies such as key positive and negative electrode materials and electrolytes. The energy density and life of the battery cells cannot meet the needs of practical applications. Therefore, it is urgent to tackle the key materials and battery cell technologies of sodium-ion batteries to promote their large-scale application.
[0003] At present, the negative electrode material of sodium batteries is mainly hard carbon. Hard carbon refers to carbon that is difficult to graphitize. It is a pyrolytic carbon obtained by pyrolysis of high molecular polymers, petrochemical products, biomass, etc. Due to the presence of a large number of heteroatoms such as H, O, and N in the precursor, the formation of crystalline regions during the heat treatment process is hindered, resulting in difficulty in graphitization even at high temperatures above 2500°C. According to the different pyrolysis and carbonization temperatures, hard carbon materials can be divided into high-temperature pyrolytic carbon between 1000-1400°C and low-temperature pyrolytic carbon between 500-1000°C. According to the different carbon sources, it can be divided into resin carbon (such as phenolic resin, epoxy resin, polyfurfuryl alcohol resin, etc.), organic polymer carbon (such as PVA, PVC, PVDF, PAN, etc.), carbon black (acetylene black prepared by CVD method, etc.), biomass carbon (such as plant residues and shells, etc.), etc.
[0004] During the pyrolysis process of hard carbon, the carbon layer tends to grow in a planar direction, but the cross-linked structure in the macromolecules hinders its growth in the planar direction. Therefore, the carbon layer in the hard carbon cannot extend infinitely to grow into a graphite-like lamellar structure. It can only form a carbon layer stacking structure in the short range and a disordered state in the long range. The hard carbon structure is mainly composed of an amorphous part. Due to the disordered stacking of some carbon layers, defects and holes appear, while the other part of the carbon layer presents a graphite microcrystalline structure. These graphite microcrystals have no orientation and are cross-linked with each other. Some researchers believe that the molecular weight of the precursor affects the microstructure of the hard carbon formed after pyrolysis. As the molecular weight increases, the degree of graphitization of the hard carbon gradually increases and the specific surface area gradually increases.
[0005] Generally, the first effect and platform capacity contribution of hard carbon are improved through closed-cell construction and surface modification, but conventional processes are difficult to achieve, or the processes are complex and costly.
[0006] Patent No. 202111433770.1 discloses a method for preparing a hard carbon composite material, comprising the following steps: (1) mixing an alkali metal fast ion conductor, a conductive agent and an organic solvent to obtain a coating material; (2) mixing a biomass raw material with an alkaline solution, filtering and drying to obtain a precursor material; (3) mixing the coating material and the solvent to obtain a coating material solution, adding the precursor material, and obtaining the composite material after carbonization treatment. Wherein: the biomass raw material includes asphalt, and the alkaline solution includes a sodium hydroxide solution; the mass ratio of sodium hydroxide in the biomass raw material and the sodium hydroxide solution is 100:(1-10). This method first removes the alkali-soluble substances in the biomass raw material with an alkali, then mixes it with an alkali metal fast ion conductor, a conductive agent and an organic solvent, adds a precursor material, and carbonizes it to obtain a hard carbon composite material. This material has not been doped, so the Coulomb efficiency is slightly low and the process flow is long.
[0007] In addition, Patent No. 202211046923.1 discloses a method for preparing a hard carbon negative electrode material by an asphalt-based cross-linking method, comprising the following steps: S1, melting and blending a powdered ion exchange resin with a powdered asphalt to obtain a molten mixture; S2, cooling and crushing the molten mixture to obtain a mixed powder;
[0008] S3, heating and carbonizing the mixed powder to obtain the hard carbon negative electrode material. This method uses asphalt and ion exchange resin to prepare a hard carbon negative electrode, which cannot form doping and has basically no pore-forming effect, and the cost of the ion exchange resin is relatively high.
[0009] Patent No. 202210544790.4 discloses a method for preparing a hard carbon negative electrode material, wherein the carbon source is subjected to high temperature pretreatment in a protective atmosphere to obtain a low-purity hard carbon powder; the low-purity hard carbon powder is acid-purified in an acid solution and then washed and dried in sequence to obtain an acid-purified hard carbon powder; the acid-purified hard carbon powder and an organic carbon source are heat-treated to obtain a single-layer coated hard carbon material; the single-layer coated hard carbon material is subjected to chemical vapor deposition in a gaseous carbon source and then screened to obtain a hard carbon negative electrode material. This method has a complex preparation process, and vapor deposition is relatively difficult to achieve large-scale production, and the cost is relatively high.
[0010] In summary, further research and development is needed on the preparation methods of hard carbon negative electrode materials to improve the first effect and platform capacity contribution of hard carbon. Summary of the invention
[0011] In order to solve the problem that it is difficult to improve the first efficiency and platform capacity contribution of hard carbon by closed-pore construction and surface modification in the above-mentioned existing processes, or that it can be achieved but the process is complicated and the cost is high, the present invention proposes a method for preparing a hard carbon negative electrode material that can form a large number of closed pores, effectively improve the coulombic efficiency, rate performance and capacity of the product and has low cost.
[0012] The present invention is achieved through the following technical solutions:
[0013] The preparation method of the above-mentioned hard carbon negative electrode material is to add asphalt to sodium hydroxide, heat it to 300-400°C in a sealed container, fully mix and dissolve it, calcine it once, crush it, mix it with organic phosphate-organic solvent, stir and disperse it, spray dry it, and then calcine it twice, crush it, screen it, and remove iron to obtain the hard carbon negative electrode material.
[0014] The preparation method of the hard carbon negative electrode material comprises the following specific steps:
[0015] 1) Add asphalt to sodium hydroxide, heat to 300-400°C in a sealed container, and mix thoroughly to dissolve;
[0016] 2) placing the dissolved mixture into a sagger for calcination, heating the mixture to 1200-1600°C at a heating rate of 2-4°C / h, keeping the temperature for 10-20h, and then cooling the mixture at a cooling rate of 2-4°C / h until the material temperature is ≤60°C, removing the mixture from the furnace, and airflow pulverizing the mixture to a particle size of 3-6μm;
[0017] 3) mixing the crushed particles with an organic phosphate-organic solvent, stirring and dispersing them, and then spray drying them;
[0018] 4) The spray-dried material is placed in a roller furnace for secondary calcination, and the material is discharged after cooling. After air flow crushing, screening, and iron removal, a hard carbon negative electrode material is obtained.
[0019] The method for preparing the hard carbon negative electrode material, wherein: in the step 1), the mass ratio of asphalt to sodium hydroxide is 1:0.1-0.3.
[0020] The preparation method of the hard carbon negative electrode material, wherein: in the step 2), during the first calcination, a roller furnace is used for calcination, and nitrogen is introduced during the calcination process for protection to maintain the oxygen content in the furnace gas below 200ppm, and the pressure in the furnace is 30-60Pa higher than the external atmospheric pressure; during the pulverization, a gas with a pressure of 0.4-0.8MPa is used for air flow pulverization.
[0021] The preparation method of the hard carbon negative electrode material, wherein: in the step 3), the organic phosphate is one or more of tributyl phosphate, di(2-ethylhexyl) phosphate, 2-ethylhexyl phosphate mono-2-ethylhexyl ester or bis(2,4,4-trimethylpentyl)phosphonic acid; the organic solvent is one or more of ethanol, n-propanol, isopropanol or ethyl acetate.
[0022] The method for preparing the hard carbon negative electrode material, wherein: in the step 3), the molar ratio of the carbon in the crushed particles to the organic phosphate is 1:0.01-0.05.
[0023] The preparation method of the hard carbon negative electrode material, wherein: in the step 3), during spray drying, stirring is performed while entering the spray drying, nitrogen is used as the air intake, and the nitrogen is heated to 150-250°C before entering the drying tower; during feeding, the atomizing wheel speed is 15000-20000r / min, and then the material is collected in the collection tower, and the exhaust gas is collected by the dust collecting bag, and the exhaust gas is condensed to recover the organic solvent, and then returned to the spray drying, and the condensed and recovered organic solution is returned for use.
[0024] The preparation method of the hard carbon negative electrode material, wherein: in the step 4), during the secondary calcination, a roller furnace is used for calcination; during the calcination process, nitrogen is introduced for protection to maintain the oxygen content in the furnace gas below 500ppm, and the pressure in the furnace is 20-40Pa higher than the external atmospheric pressure.
[0025] The method for preparing the hard carbon negative electrode material, wherein: in the step 4), the gas flow is crushed with a pressure of 0.4-0.8 MPa to crush the material to a particle size of 5-15 μm.
[0026] The preparation method of the hard carbon negative electrode material, wherein: during the primary calcination and the secondary calcination, an exhaust port is provided in the temperature rising section, the exhaust port is connected to the induced draft fan, the induced draft fan is connected to the spray absorption tower, and pure water is used for spray absorption to obtain a first spray absorption liquid and a second spray absorption liquid respectively.
[0027] Beneficial effects:
[0028] 1. The present invention cleverly utilizes the principle that asphalt and sodium hydroxide can dissolve in each other. After dissolving in each other at a certain temperature, they are carbonized at high temperature, and the dissolved sodium hydroxide will evaporate, forming a large number of pores in the material after the asphalt carbonization. Then, organic phosphate-organic solvent is mixed and spray-dried, and the organic phosphate is adsorbed into the pores. After secondary carbonization, a large number of open pores are converted into closed pores, thereby forming a large number of closed pores, which is conducive to the embedding of sodium and avoids the deposition of sodium on the hard carbon surface.
[0029] 2. The present invention introduces organic phosphate in the second step, part of the phosphorus element will volatilize, and part of the phosphorus will form some CPO bonds with carbon, thereby improving the coulombic efficiency, rate performance and capacity of the product.
[0030] 3. The present invention uses asphalt as raw material, which has low cost and high residual carbon rate, and the carbon BET produced by asphalt is small. The hard carbon obtained by carbonization and decomposition of organic phosphate has a low residual carbon rate and a small carbon BET, and is doped with phosphorus, which can be conveniently adsorbed and ion transported.
[0031] 4. The product prepared by the present invention has high capacity, high coulombic efficiency and good cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The charge and discharge curve of the hard carbon negative electrode material prepared in Example 1 of the present invention;
[0033] Figure 2 This is a SEM image of the hard carbon negative electrode material prepared in Example 1 of the present invention;
[0034] Figure 3 This is a charge and discharge curve diagram of the hard carbon negative electrode material prepared in Example 5 of the present invention. DETAILED DESCRIPTION
[0035] The preparation method of the hard carbon negative electrode material of the present invention is to add asphalt to sodium hydroxide, heat to 300-400°C in a sealed container, fully mix and dissolve, calcine once, crush, mix organic phosphate-organic solvent, spray dry after stirring and dispersion, and then calcine twice, crush, screen, and remove iron to obtain the hard carbon negative electrode material. After the asphalt and sodium hydroxide are dissolved in each other, they are carbonized at high temperature, and the dissolved sodium hydroxide will volatilize, forming a large number of pores in the material after the asphalt is carbonized; then the organic phosphate-organic solvent is mixed, and after spray drying, the organic phosphate will be adsorbed into the pores; after secondary carbonization, a large number of open pores are converted into closed pores, thereby forming a large number of closed pores, which is conducive to the embedding of sodium and avoids the deposition of sodium on the hard carbon surface.
[0036] The preparation method of the hard carbon negative electrode material of the present invention comprises the following specific steps:
[0037] 1) Add asphalt to sodium hydroxide, heat to 300-400°C in a sealed container, and mix thoroughly to dissolve;
[0038] 2) placing the dissolved mixture into a sagger for calcination, heating the mixture to 1200-1600°C at a heating rate of 2-4°C / h, keeping the temperature for 10-20h, and then cooling the mixture at a cooling rate of 2-4°C / h until the material temperature is ≤60°C, removing the mixture from the furnace, and airflow pulverizing the mixture to a particle size of 3-6μm;
[0039] 3) mixing the crushed particles with an organic phosphate-organic solvent, stirring and dispersing them, and then spray drying them;
[0040] 4) The spray-dried material is placed in a roller furnace for secondary calcination, and the material is discharged after cooling. After air flow crushing, screening, and iron removal, a hard carbon negative electrode material is obtained.
[0041] In step 1), the mass ratio of asphalt to sodium hydroxide is 1:0.1-0.3.
[0042] In step 2), during the primary calcination, a roller furnace is used for calcination, and nitrogen is introduced for protection during the calcination process to maintain the oxygen content in the gas in the furnace below 200ppm, and the pressure in the furnace is 30-60Pa higher than the external atmospheric pressure; an exhaust port is provided in the temperature rising section, the exhaust port is connected to the induced draft fan, the induced draft fan is connected to the spray absorption tower, and pure water is used for spray absorption to obtain a first spray absorption liquid;
[0043] During the pulverization, gas with a pressure of 0.4-0.8 MPa is used for air flow pulverization, and then classification is performed to obtain pulverized particles.
[0044] In step 3), the organic phosphate is one or more of tributyl phosphate, di(2-ethylhexyl) phosphate, 2-ethylhexyl phosphate mono-2-ethylhexyl ester or bis(2,4,4-trimethylpentyl)phosphonic acid; the organic solvent is one or more of ethanol, n-propanol, isopropanol or ethyl acetate;
[0045] During spray drying, the material is stirred while entering the spray drying. Nitrogen is used as the inlet gas, and the nitrogen is heated to 150-250℃ before entering the drying tower. During feeding, the speed of the atomizing wheel is 15000-20000r / min, and then the material is collected in the collection tower. After the waste gas passes through the dust collecting bag for dust collection, the waste gas is condensed to recover the organic solvent, and then returned to the spray drying, and the condensed and recovered organic solution is returned for use;
[0046] The molar ratio of carbon to organic phosphate in the crushed particles is 1:0.01-0.05.
[0047] In step 4), during the secondary calcination, a roller furnace is used for calcination; during the calcination process, nitrogen is introduced for protection to maintain the oxygen content in the furnace gas below 500ppm, and the pressure in the furnace is 20-40Pa higher than the external atmospheric pressure; an exhaust port is provided in the temperature rising section, the exhaust port is connected to the induced draft fan, the induced draft fan is connected to the spray absorption tower, and pure water is used for spray absorption to obtain a second spray absorption liquid;
[0048] During the crushing process, a gas pressure of 0.4-0.8 MPa is used for air flow crushing, and the material is crushed to a particle size of 5-15 μm;
[0049] After sieving through a 20-80 mesh sieve and removing iron, the product is vacuum packed. The packaging is carried out in a constant temperature and humidity room with a temperature of 20±5℃ and a humidity of ≤10%.
[0050] The present invention is further described below with reference to specific embodiments.
[0051] Example 1
[0052] Add asphalt to sodium hydroxide, with the mass ratio of asphalt to sodium hydroxide being 1:0.2; then heat to 330°C in a sealed container and mix thoroughly to dissolve;
[0053] The dissolved mixture is placed in a sagger for calcination. A roller furnace is used for calcination. Nitrogen is introduced during the calcination process for protection. The oxygen content in the gas in the furnace is maintained below 200ppm. The pressure in the furnace is 45Pa higher than the external atmospheric pressure. The temperature is raised to 1400°C at a rate of 3°C / h, kept at that temperature for 15h, and then cooled to a material temperature of 55°C at a cooling rate of 3°C / h. The mixture is then taken out of the furnace and air flow crushed to a particle size of 4.5μm using a gas at a pressure of 0.65MPa.
[0054] The crushed particles are mixed with tributyl phosphate and n-propanol, wherein the molar ratio of carbon in the crushed particles to tributyl phosphate is 1:0.03; the particles are spray dried while being stirred, nitrogen is used as the inlet gas, and the nitrogen is heated to 200°C before entering the drying tower. During feeding, the speed of the atomizing wheel is 18000r / min, and the materials are collected in the collecting tower. After the waste gas passes through the dust collecting bag for dust collection, the waste gas is condensed to recover the organic solvent, and then returned to the spray dryer, and the condensed and recovered organic solution is returned for use;
[0055] The spray-dried material is placed in a roller furnace for secondary calcination, and nitrogen is introduced for protection to maintain the oxygen content in the furnace gas below 500ppm. The pressure in the furnace is 30Pa higher than the external atmospheric pressure, and the material is discharged after cooling; it is airflow-pulverized by gas with a pressure of 0.65MPa to a particle size of 10.3μm; it is sieved through a 50-mesh sieve, and vacuum-packed after iron removal to obtain a hard carbon negative electrode material; the packaging is carried out in a constant temperature and humidity room with a temperature of 25°C and a humidity of 9.6%.
[0056] During the primary calcination and the secondary calcination, an exhaust port is provided in the temperature rising section, the exhaust port is connected to the induced draft fan, the induced draft fan is connected to the spray absorption tower, and pure water is used for spray absorption to obtain the first spray absorption liquid and the second spray absorption liquid respectively.
[0057] The hard carbon negative electrode material finally prepared has test data as shown in Table 1 and charge and discharge curves as shown in Figure 1The charge and discharge curve adopts the buckle test. The sample, acetylene black and CMC are mixed in a mass ratio of 8:1:1, coated on copper foil, vacuum dried at 80℃ for more than 8h, punched, and assembled with glass fiber diaphragm and sodium hexafluorophosphate electrolyte (1mol / L NaPF6 in DIGLYME=100Vol%) into the buckle test. The buckle assembly method for testing other embodiments is consistent with that in embodiment 1, and the test voltage range is 0-3V.
[0058] Table 1 Test data of hard carbon negative electrode material prepared in Example 1
[0059]
[0060] SEM Figure 2 ,from Figure 2 It is granular and has a wide primary particle size distribution.
[0061] Example 2
[0062] Add asphalt to sodium hydroxide, with the mass ratio of asphalt to sodium hydroxide being 1:0.1; then heat to 300°C in a sealed container and mix thoroughly to dissolve;
[0063] The dissolved mixture is placed in a sagger for calcination. A roller furnace is used for calcination. Nitrogen is introduced during the calcination process for protection. The oxygen content in the gas in the furnace is maintained below 200ppm. The pressure in the furnace is 30Pa higher than the external atmospheric pressure. The temperature is raised to 1200°C at a rate of 2°C / h, kept at that temperature for 10h, and then cooled to a material temperature of 58°C at a cooling rate of 2°C / h. The mixture is then taken out of the furnace and air flow crushed to a particle size of 3μm using a gas at a pressure of 0.4MPa.
[0064] The crushed particles are mixed with 2-ethylhexyl mono-2-ethylhexyl phosphate or bis(2,4,4-trimethylpentyl)phosphonic acid and isopropanol, wherein the molar ratio of carbon in the crushed particles to tributyl phosphate is 1:0.01; the particles are spray dried while being stirred, nitrogen is used as the inlet gas, and the nitrogen is heated to 150° C. before entering the drying tower. During feeding, the speed of the atomizing wheel is 15000 r / min, and the materials are collected in the collecting tower. After the waste gas is collected by a dust collecting bag, the waste gas is condensed to recover the organic solvent, and then returned to the spray dryer, and the condensed and recovered organic solution is returned for use;
[0065] The spray-dried material is placed in a roller furnace for secondary calcination, and nitrogen is introduced for protection to maintain the oxygen content in the furnace gas below 500ppm. The pressure in the furnace is 20Pa higher than the external atmospheric pressure, and the material is discharged after cooling; it is airflow-pulverized by gas with a pressure of 0.4MPa to a particle size of 5μm; it is sieved through an 80-mesh sieve, and vacuum-packed after iron removal to obtain a hard carbon negative electrode material; the packaging is carried out in a constant temperature and humidity room with a temperature of 15°C and a humidity of 9%.
[0066] During the primary calcination and the secondary calcination, an exhaust port is provided in the temperature rising section, the exhaust port is connected to the induced draft fan, the induced draft fan is connected to the spray absorption tower, and pure water is used for spray absorption to obtain the first spray absorption liquid and the second spray absorption liquid respectively.
[0067] The test data of the hard carbon negative electrode material finally prepared are shown in Table 2.
[0068] Table 2 Test data of hard carbon negative electrode material prepared in Example 2
[0069]
[0070] Example 3
[0071] Add asphalt to sodium hydroxide, with the mass ratio of asphalt to sodium hydroxide being 1:0.3; then heat to 400°C in a sealed container and mix thoroughly to dissolve;
[0072] The dissolved mixture is placed in a sagger for calcination. A roller furnace is used for calcination. Nitrogen is introduced during the calcination process for protection. The oxygen content in the gas in the furnace is maintained below 200ppm. The pressure in the furnace is 60Pa higher than the external atmospheric pressure. The temperature is raised to 1600°C at a rate of 4°C / h, kept at that temperature for 20h, and then cooled to a material temperature of 60°C at a cooling rate of 4°C / h. The mixture is then taken out of the furnace and pulverized with gas at a pressure of 0.8MPa to a particle size of 6μm.
[0073] The crushed particles are mixed with di(2-ethylhexyl) phosphate and ethyl acetate, wherein the molar ratio of carbon in the crushed particles to tributyl phosphate is 1:0.05; the particles are spray dried while being stirred, nitrogen is used as the inlet gas, and the nitrogen is heated to 250°C before entering the drying tower. During feeding, the speed of the atomizing wheel is 20000r / min, and the materials are collected in the collecting tower. After the waste gas passes through the dust collecting bag for dust collection, the waste gas is condensed to recover the organic solvent, and then returned to the spray dryer, and the condensed and recovered organic solution is returned for use;
[0074] The spray-dried material is placed in a roller furnace for secondary calcination, and nitrogen is introduced for protection to maintain the oxygen content in the furnace gas below 500ppm. The pressure in the furnace is 40Pa higher than the external atmospheric pressure, and the material is discharged after cooling; it is airflow-pulverized by gas with a pressure of 0.8MPa to a particle size of 15μm; it is sieved through a 20-mesh sieve, vacuum-packed after iron removal, and a hard carbon negative electrode material is obtained; the packaging is carried out in a constant temperature and humidity room with a temperature of 20°C and a humidity of 10%.
[0075] During the primary calcination and the secondary calcination, an exhaust port is provided in the temperature rising section, the exhaust port is connected to the induced draft fan, the induced draft fan is connected to the spray absorption tower, and pure water is used for spray absorption to obtain the first spray absorption liquid and the second spray absorption liquid respectively.
[0076] The test data of the hard carbon negative electrode material finally prepared are shown in Table 3.
[0077] Table 3 Test data of hard carbon negative electrode material prepared in Example 3
[0078]
[0079] Example 4
[0080] Add asphalt to sodium hydroxide, with the mass ratio of asphalt to sodium hydroxide being 1:0.25; then heat to 380°C in a sealed container and mix thoroughly to dissolve;
[0081] The dissolved mixture is placed in a sagger for calcination. A roller furnace is used for calcination. Nitrogen is introduced during the calcination process for protection. The oxygen content in the gas in the furnace is maintained below 200ppm. The pressure in the furnace is 50Pa higher than the external atmospheric pressure. The temperature is raised to 1500°C at a rate of 3.5°C / h, kept at that temperature for 12h, and then cooled to a material temperature of 58°C at a cooling rate of 3.5°C / h. The mixture is then taken out of the furnace and air flow crushed to a particle size of 4μm using a gas with a pressure of 0.5MPa.
[0082] The crushed particles are mixed with tributyl phosphate, di(2-ethylhexyl) phosphate and ethanol; wherein the molar ratio of carbon in the crushed particles to tributyl phosphate and di(2-ethylhexyl) phosphate is 1:0.04; the particles are spray dried while being stirred, nitrogen is used as the inlet gas, and the nitrogen is heated to 200° C. before entering the drying tower. During feeding, the speed of the atomizing wheel is 17000 r / min, and the materials are collected in the collecting tower. After the waste gas is collected by a dust collecting bag, the waste gas is condensed to recover the organic solvent, and then returned to the spray dryer, and the condensed and recovered organic solution is returned for use;
[0083] The spray-dried material is placed in a roller furnace for secondary calcination, and nitrogen is introduced for protection to maintain the oxygen content in the furnace gas below 500ppm. The pressure in the furnace is 30Pa higher than the external atmospheric pressure, and the material is discharged after cooling; it is airflow-pulverized by gas at a pressure of 0.5MPa to a particle size of 12.3μm; it is sieved through a 60-mesh sieve, and vacuum-packed after iron removal to obtain a hard carbon negative electrode material; the packaging is carried out in a constant temperature and humidity room with a temperature of 23°C and a humidity of 9.2%.
[0084] During the primary calcination and the secondary calcination, an exhaust port is provided in the temperature rising section, the exhaust port is connected to the induced draft fan, the induced draft fan is connected to the spray absorption tower, and pure water is used for spray absorption to obtain the first spray absorption liquid and the second spray absorption liquid respectively.
[0085] The test data of the hard carbon negative electrode material finally prepared are shown in Table 4.
[0086] Table 4 Test data of hard carbon negative electrode material prepared in Example 4
[0087]
[0088] Example 5
[0089] Add asphalt to sodium hydroxide, with the mass ratio of asphalt to sodium hydroxide being 1:0.3; then heat to 350°C in a sealed container and mix thoroughly to dissolve;
[0090] The dissolved mixture is placed in a sagger for calcination. A roller furnace is used for calcination. Nitrogen is introduced during the calcination process for protection. The oxygen content in the gas in the furnace is maintained below 200ppm. The pressure in the furnace is 40Pa higher than the external atmospheric pressure. The temperature is raised to 1500°C at a rate of 3°C / h, kept at that temperature for 18h, and then cooled to a material temperature of 55°C at a cooling rate of 3°C / h. The mixture is then taken out of the furnace and pulverized with gas at a pressure of 0.7MPa to a particle size of 5μm.
[0091] The crushed particles are mixed with tributyl phosphate, ethanol and n-propanol; wherein the molar ratio of carbon in the crushed particles to tributyl phosphate is 1:0.03; the particles are spray dried while being stirred, nitrogen is used as the inlet gas, and the nitrogen is heated to 230°C before entering the drying tower. During feeding, the speed of the atomizing wheel is 19000r / min, and the materials are collected in the collecting tower. After the waste gas passes through the dust collecting bag for dust collection, the waste gas is condensed to recover the organic solvent, and then returned to the spray dryer, and the condensed and recovered organic solution is returned for use;
[0092] The spray-dried material is placed in a roller furnace for secondary calcination, and nitrogen is introduced for protection to maintain the oxygen content in the furnace gas below 500ppm. The pressure in the furnace is 35Pa higher than the external atmospheric pressure, and the material is discharged after cooling; it is airflow-pulverized by gas with a pressure of 0.7MPa to a particle size of 8.4μm; it is sieved through a 70-mesh sieve, and vacuum-packed after iron removal to obtain a hard carbon negative electrode material; the packaging is carried out in a constant temperature and humidity room with a temperature of 21°C and a humidity of 9.3%.
[0093] During the primary calcination and the secondary calcination, an exhaust port is provided in the temperature rising section, the exhaust port is connected to the induced draft fan, the induced draft fan is connected to the spray absorption tower, and pure water is used for spray absorption to obtain the first spray absorption liquid and the second spray absorption liquid respectively.
[0094] The test data of the hard carbon negative electrode material finally prepared are shown in Table 5.
[0095] Table 5 Test data of hard carbon negative electrode material prepared in Example 5
[0096]
[0097] At the same time, the rate performance of the material of Example 5 was tested. The buckle battery prepared from the material of Example 5 was tested at 1C / 2C / 3C / 4C and 5C respectively. The charge and discharge curves are as follows: Figure 3 As shown, its rate performance is relatively excellent.
Claims
1. A method for preparing a hard carbon negative electrode material, characterized in that: 1) Add asphalt to sodium hydroxide, heat to 300-400℃ in a sealed container, mix and dissolve thoroughly; 2) Put the dissolved mixture into a sagger for calcination, heat to 1200-1600℃ at a heating rate of 2-4℃ / h, keep warm for 10-20h, then cool at a cooling rate of 2-4℃ / h until the material temperature is ≤60℃ After that, it is taken out of the furnace and air flow crushed to a particle size of 3-6μm. During the first calcination, a roller furnace is used for calcination. Nitrogen is introduced for protection during the calcination process to maintain the oxygen content in the furnace gas below 200ppm. The pressure in the furnace is 30-60Pa higher than the external atmospheric pressure. During crushing, a gas with a pressure of 0.4-0.8MPa is used for air flow crushing; 3) the crushed particles are mixed with an organic phosphate-organic solvent, stirred and dispersed, and then spray dried; 4) the spray-dried material is then calcined for the second time, and the material is discharged after cooling. After air flow crushing, screening, and iron removal, a hard carbon negative electrode material is obtained; during the second calcination, a roller furnace is used for calcination; during the calcination process, nitrogen is introduced for protection to maintain the oxygen content in the furnace gas below 500ppm, and the pressure in the furnace is 20-40Pa higher than the external atmospheric pressure; the mass ratio of asphalt to sodium hydroxide is 1:0.1-0.3, and the ratio of the molar number of carbon in the crushed particles to the organic phosphate is 1:0.01-0.
05.
2. The method for preparing the hard carbon negative electrode material according to claim 1, characterized in that: In the step 3), the organic phosphate is one or more of tributyl phosphate, di(2-ethylhexyl) phosphate, 2-ethylhexyl phosphate mono-2-ethylhexyl ester or bis(2,4,4-trimethylpentyl)phosphonic acid; and the organic solvent is one or more of ethanol, n-propanol, isopropanol or ethyl acetate.
3. The method for preparing the hard carbon negative electrode material according to claim 1, characterized in that: In the step 3), during spray drying, stirring is performed while entering the spray drying, nitrogen is used as the air intake, and the nitrogen is heated to 150-250° C. before entering the drying tower; during feeding, the speed of the atomizing wheel is 15000-20000 r / min, and then the material is collected in the collection tower, and the waste gas is collected by the dust collecting bag, and the waste gas is condensed to recover the organic solvent, and then returned to the spray drying, and the condensed and recovered organic solution is returned for use.
4. The method for preparing the hard carbon negative electrode material according to claim 1, characterized in that: In the step 4), the gas with a pressure of 0.4-0.8 MPa is used for air flow pulverization, and the material is pulverized to a particle size of 5-15 μm.
5. The method for preparing the hard carbon negative electrode material according to claim 1, characterized in that: During the primary calcination and the secondary calcination, an exhaust port is provided in the temperature rising section, the exhaust port is connected to the induced draft fan, the induced draft fan is connected to the spray absorption tower, and pure water is used for spray absorption to obtain the first spray absorption liquid and the second spray absorption liquid respectively.