A ceramsite prepared by using sludge anaerobic digestion residue and its preparation method and application

By preparing ceratops of sludge anaerobic digestion residue with fly ash and clay, the environmental pollution problem in the treatment of sludge anaerobic digestion residues is solved, and the resource utilization and catalytic performance are improved, providing a clean, Economical water treatment method.

CN116874281BActive Publication Date: 2024-12-06DALIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310963635.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-02
Publication Date
2024-12-06
Estimated Expiration
2043-08-02

AI Technical Summary

Technical Problem

Treatment methods of anaerobic digestion of sludge residues such as landfill and incineration have problems of environmental pollution and resource waste, and have failed to achieve stable and resource-based reduction treatment.

Method used

Ceramic granules are prepared by anaerobic digestion residues, fly ash and clay as the main raw materials. Ceramic granules with catalytic properties are prepared by drying, grinding, mixing, granulation, sintering and other steps, for water treatment and Ozone catalysis.

Benefits of technology

The resource utilization of anaerobic digested residue of sludge has been realized. The prepared ceramic granules have low wear rate, low heavy metal leaching toxicity, excellent catalytic performance and environmentally friendly water treatment filter performance, meeting the needs of the sewage treatment field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116874281B_ABST
    Figure CN116874281B_ABST
Patent Text Reader

Abstract

The present invention provides ceramsite, a method for preparing ceramsite using sludge anaerobic digestion residue, and an application method thereof. The raw material composition of ceramsite is 45%-51% of sludge anaerobic digestion residue, 30%-34% of fly ash, and 15%-25% of clay. The sintering process of sludge biogas residue-based ceramsite is: preheating temperature 350°C, preheating time 25min, sintering temperature 1050°C, and preheating time 10min. The process includes drying; grinding and screening; weighing and mixing; granulation; drying; and firing ceramsite. The present invention prepares ceramsite using sludge anaerobic digestion residue, reduces the pollution problem of sludge anaerobic digestion residue to the environment, and also realizes the resource utilization of sludge anaerobic digestion residue, greatly reducing the treatment cost of sludge anaerobic digestion residue and the preparation cost of ceramsite. Even the prepared ceramsite can bring certain benefits. The ceramsite prepared from sludge anaerobic digestion residue can be used as a catalyst for advanced oxidation reaction to improve oxidation efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to reducing, harmless and resourceful treatment of anaerobic digestion residues of sludge, and in particular to ceramsite prepared from anaerobic digestion residues of sludge, and a preparation method and application thereof. Background Art

[0002] With the rapid development of urbanization, the discharge of urban sewage has continued to increase, and the byproduct of sewage treatment - residual sludge has also increased. The treatment and disposal of residual sludge includes landfill, incineration, anaerobic digestion, composting and use as building materials. Based on the characteristics of high efficiency of nutrient recycling and low environmental impact of anaerobic digestion, sludge anaerobic digestion to produce methane (sludge biogasification) has become one of the main treatment methods for industrial sludge reduction. However, while the current sludge biogasification project is vigorously developing, a large amount of sludge anaerobic digestion residues are produced.

[0003] As a by-product of anaerobic digestion of sludge, the residue of anaerobic digestion of sludge contains a variety of nutrients (such as nitrogen and phosphorus) and a large amount of harmful substances (such as pathogenic microorganisms and heavy metals). For example, the components in the residue of anaerobic digestion of sludge reported in the literature [Monlau, F., Sambusiti, C., Ficara, E., Aboulkas, A., Barakat, A., Carrère, H., 2015. New opportunities for agricultural digestate valorization: current situation and perspectives. Energ. Environ. Sci. 8, 26-2621] pose a threat to human health and the environment. The treatment of anaerobic sludge digestion residues mainly adopts the methods of stacking landfill and drying incineration, such as the disposal methods of anaerobic sludge digestion residues reported in the literature [De Corato, U., De Bari, I., Viola, E., Pugliese, M., 2018. Assessing the main opportunities of integrated biorefining from agro-bioenergy co / by-products and agroindustrial residues into high-value added products associated to some emerging markets: Areview. Renew. Sust. Energ. Rev. 88, 326-346]. After the anaerobic digestion residue of sludge is landfilled, the organic matter in it will ferment and produce foul-smelling gas and escape, and the heavy metal substances in it will also enter the soil with the leachate, causing secondary pollution to the surrounding environment, such as the landfill treatment of anaerobic digestion residue of sludge reported in the literature [Yaashikaa, PR, Kumar, PS, Nhung, TC, Hemavathy, RV, Jawahar, MJ, Neshaanthini, JP, Rangasamy, G., 2022. A review on landfill system for municipal solid wastes: Insight into leachate, gas emissions, environmental and economic analysis. Chemosphere 309, 136627].Incineration will transfer a large amount of heavy metal substances in the anaerobic digestion residue of sludge to the ash, which will exist in the form of other solid wastes and continue to cause harm to the environment, such as the incineration treatment of anaerobic digestion residues of sludge reported in the literature [Zeng, Q., Zhen, S., Liu, J., Ni, Z., Chen, J., Liu, Z., Qi, C., 2022. Impact of solid digestate processing on carbon emission of an industrial-scale food waste codigestion plant. Bioresour. Technol. 360, 127639]. Therefore, the common methods of anaerobic digestion residue disposal such as landfill and drying incineration are only temporary solutions, which only transfer the space where pollution occurs or delay the time of pollution occurrence, and cannot achieve the purpose of stabilizing and resource-based disposal of huge amounts of anaerobic digestion residues of sludge. In order to solve this problem, it is crucial to develop technologies that can stabilize and recycle at the same time.

[0004] Due to its advantages such as low wear rate, large specific surface area, high porosity and strong acid and alkali resistance, expanded clay is often used as water treatment filter material. The traditional raw materials for expanded clay production are mainly natural resource materials such as clay and shale. The mining of large amounts of natural resource materials not only affects the natural environment, but also poses a huge threat to the depletion of natural resources. The technology of developing and utilizing recyclable materials or solid waste materials as raw materials for ceramsite has attracted more and more attention. For example, a Chinese invention patent (application publication number: CN112573901A) discloses a method for preparing homogeneous porous ceramsite using sludge, comprising: 1) weighing raw materials by weight: 20 to 70 parts of sludge, 0 to 20 parts of fly ash, 20 to 75 parts of building waste, and 0.2% to 4% of silicon carbide based on the total weight of sludge, fly ash and building waste; mixing sludge, optional fly ash, building waste, silicon carbide and water to obtain a mixed slurry; 2) wet ball milling the mixed slurry, separating it, and obtaining a ball-milled material; 3) granulating the ball-milled material into balls to obtain ceramsite green balls; 4) drying and sintering the ceramsite green balls to obtain homogeneous porous ceramsite.

[0005] The anaerobic digestion residue of sludge is used as the raw material for preparing ceramsite, and the anaerobic digestion residue-based ceramsite of sludge is fired, and these inorganic components are fixed in the anaerobic digestion residue-based ceramsite, in order to realize the resource utilization of solid residue. O3 is widely used in the deep treatment of wastewater due to its strong oxidizing property, and its oxidation performance needs to be improved by the use of catalysts. There is no lack of metal elements with catalytic properties (such as iron from coagulated sludge) in the inorganic substances fixed in the anaerobic digestion residue-based ceramsite of sludge. Ozone can react with iron oxides on the surface of the catalyst. Therefore, the anaerobic digestion residue-based ceramsite of sludge has the potential to be used as water treatment filter ceramsite for O3 catalysis. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing ceramsite by utilizing anaerobic digestion residue of sludge in combination with other materials, which can reduce the amount of anaerobic digestion residue of sludge, render it harmless and recycle it, reduce its harm to the environment, realize the resource utilization of solid waste and turn waste into treasure.

[0007] The technical solution of the present invention:

[0008] The invention discloses ceramsite, wherein the raw materials of the ceramsite are composed of 45%-51% of sludge anaerobic digestion residue, 30%-34% of fly ash and 15%-25% of clay in terms of weight percentage.

[0009] Furthermore, the raw material composition of the sludge biogas residue-based ceramsite is: 51% sludge anaerobic digestion residue, 34% fly ash, and 5% clay.

[0010] Furthermore, the anaerobic digestion residue of the sludge is the sieve-down obtained by drying the anaerobic digestion residue of the sludge, grinding it manually and screening it with a 100-mesh sieve.

[0011] Furthermore, the fly ash is fly ash powder that is dried, manually ground, and sieved through a 100-mesh sieve to obtain the undersize.

[0012] Furthermore, the clay is clay powder that is dried, manually ground, and sieved through a 100-mesh sieve to obtain the undersize.

[0013] A method for preparing ceramsite using sludge anaerobic digestion residue, the steps are as follows:

[0014] S1 Raw material drying: Place the sludge anaerobic digestion residue in a blast drying oven and dry it at a temperature of 105°C to make its mass moisture content less than 5%;

[0015] S2 raw material grinding: putting the anaerobic digestion residue of sludge dried in step S1 into a grinder for grinding, passing the ground anaerobic digestion residue powder through a 100-mesh sieve, and taking the sieve residue and saving it for later use;

[0016] S3 weighing, stirring and mixing: weighing a certain amount of the sludge anaerobic digestion residue powder, fly ash powder and clay powder dried in step S2 according to the mass percentage, putting the weighed three raw material powders into the same container, and mixing them under the action of a fast mixer for later use;

[0017] S4 granulation and balling: adding the raw material powder mixed in step S3 until the moisture content is 20%-35%, using a granulator to make balls, and obtaining raw material balls with a particle size of 6 mm;

[0018] S5: drying the raw balls: placing the raw balls prepared in step S4 into a blast drying oven and drying them at 105°C for 6 hours;

[0019] S6 high temperature sintering: the raw material balls dried in step S5 are placed in a box-type resistance furnace, first preheated at 350°C for 25 minutes, then heated to 1050°C and sintered for 10 minutes. After the sintering is completed, the power is turned off and the balls are naturally cooled to room temperature to obtain sludge anaerobic digestion residue-based ceramsite.

[0020] Furthermore, the different raw materials in step S3 are fully mixed, which is more conducive to the eutectic formation of SiO2 and Al2O3 in the raw materials, and more conducive to the fixation of heavy metal substances in the anaerobic digestion residue of sludge in the eutectic framework of SiO2 and Al2O3;

[0021] The anaerobic digestion residue of the sludge contains high concentrations of different transition metals, such as iron from the coagulated sludge.

[0022] A method for preparing ceramsite from sludge anaerobic digestion residue. The prepared ceramsite can be used as an ozone catalyst in the process of deep treatment of phenol-containing wastewater.

[0023] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention uses sludge anaerobic digestion residue as the main raw material to prepare ceramsite, develops a new resource utilization method for sludge anaerobic digestion residue, and prepares high-physical performance ceramsite that can be used as an ozone catalyst. The ceramsite based on sludge anaerobic digestion residue has the characteristics of low wear rate, low apparent density, large specific surface area and rich pore structure, and all performance indicators are better than the requirements of the Chinese industry standard CJ / T 299-2008. At the same time, sludge anaerobic digestion residue-based ceramsite has been proven to be an effective ozone catalyst, showing excellent catalytic performance. The heavy metal leaching toxicity of solid residue-based ceramsite is much lower than the requirements of the Chinese national standard GB 5085.3-2007, and can be used as an environmentally friendly water treatment filter material in the field of sewage treatment. In summary, this study provides a more novel, cleaner and more economical way for the treatment and disposal of solid residues, and has great research value. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1Process flow chart for preparing ceramsite from the residue of anaerobic digestion of sludge in Example 1. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. The embodiments described in the present invention are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present invention.

[0026] Example 1

[0027] The present embodiment provides a method for preparing ceramsite using sludge anaerobic digestion residue, which specifically comprises the following raw materials in weight percentage: 45% sludge anaerobic digestion residue, 30% fly ash, and 25% clay.

[0028] This embodiment also provides a method for preparing ceramsite using sludge anaerobic digestion residue, comprising the following steps:

[0029] S1 Raw material drying: Put the anaerobic digestion residue of sludge with a mass moisture content of 78% into a blast drying oven and dry the moisture at a temperature of 105°C to make its mass moisture content less than 5%;

[0030] S2 raw material grinding: putting the anaerobic digestion residue of sludge dried in step S1 into a grinder for grinding, passing the ground anaerobic digestion residue powder through a 100-mesh sieve, and taking the sieve residue and saving it for later use;

[0031] S3 weighing, stirring and mixing: weighing a certain amount of the sludge anaerobic digestion residue powder, fly ash powder and clay powder dried in step S2 according to the mass percentage, putting the weighed three raw material powders into the same container, and mixing them under the action of a fast mixer for later use;

[0032] S4 granulation and balling: add appropriate amount of water to the raw material powder mixed in step S3 to make its moisture content 30%, use a granulator to make balls, and obtain raw material balls with a particle size of 6 mm;

[0033] S5: drying the raw material balls: placing the raw material balls prepared in step S4 into a blast drying oven and drying them at 105°C for 8 hours;

[0034] S6 high temperature sintering: put the raw material balls dried in step S5 into a box-type resistance furnace, preheat at 350°C for 25 minutes at a heating rate of 10°C / min, then heat to 1050°C and sinter for 10 minutes. After sintering, turn off the power and cool naturally to room temperature to obtain finished sludge anaerobic digestion residue-based expanded clay.

[0035] Example 2

[0036] The present embodiment provides a method for preparing ceramsite using anaerobic digestion residue of sludge. Specifically, the method comprises the following raw materials in weight percentage: 48% anaerobic digestion residue of sludge, 32% fly ash, and 20% clay.

[0037] This embodiment also provides a method for preparing ceramsite using sludge anaerobic digestion residue, comprising the following steps:

[0038] S1 Raw material drying: Put the anaerobic digestion residue of sludge with a mass moisture content of 78% into a blast drying oven and dry the moisture at a temperature of 105°C to make its mass moisture content less than 5%;

[0039] S2 raw material grinding: putting the anaerobic digestion residue of sludge dried in step S1 into a grinder for grinding, passing the ground anaerobic digestion residue powder through a 100-mesh sieve, and taking the sieve residue and saving it for later use;

[0040] S3 weighing, stirring and mixing: weighing a certain amount of the sludge anaerobic digestion residue powder, fly ash powder and clay powder dried in step S2 according to the mass percentage, putting the weighed three raw material powders into the same container, and mixing them under the action of a fast mixer for later use;

[0041] S4 granulation and balling: add appropriate amount of water to the raw material powder mixed in step S3 to make its moisture content 35%, use a granulator to make balls, and obtain raw material balls with a particle size of 6 mm;

[0042] S5: drying the raw balls: placing the raw balls prepared in step S4 into a blast drying oven and drying them at 105°C for 4 hours;

[0043] S6 high temperature sintering: put the raw material balls dried in step S5 into a box-type resistance furnace, preheat at 350°C for 25 minutes at a heating rate of 10°C / min, then heat to 1050°C and sinter for 10 minutes. After sintering, turn off the power and cool naturally to room temperature to obtain finished sludge anaerobic digestion residue-based expanded clay.

[0044] Example 3

[0045] The present embodiment provides a method for preparing ceramsite using sludge anaerobic digestion residue, which specifically comprises the following raw materials in weight percentage: 51% sludge anaerobic digestion residue, 34% fly ash, and 15% clay.

[0046] This embodiment also provides a method for preparing ceramsite using sludge anaerobic digestion residue, comprising the following steps:

[0047] S1 Raw material drying: Put the anaerobic digestion residue of sludge with a mass moisture content of 78% into a blast drying oven and dry the moisture at a temperature of 105°C to make its mass moisture content less than 5%;

[0048] S2 raw material grinding: putting the anaerobic digestion residue of sludge dried in step S1 into a grinder for grinding, passing the ground anaerobic digestion residue powder through a 100-mesh sieve, and taking the sieve residue and saving it for later use;

[0049] S3 weighing, stirring and mixing: weighing a certain amount of the sludge anaerobic digestion residue powder, fly ash powder and clay powder dried in step S2 according to the mass percentage, putting the weighed three raw material powders into the same container, and mixing them under the action of a fast mixer for later use;

[0050] S4 granulation and balling: add appropriate amount of water to the raw material powder mixed in step S3 to make its moisture content 25%, use a granulator to make balls, and obtain raw material balls with a particle size of 6 mm;

[0051] S5: drying the raw balls: placing the raw balls prepared in step S4 into a blast drying oven and drying them at 105°C for 6 hours;

[0052] S6 high temperature sintering: the raw material balls dried in step S5 are placed in a box-type resistance furnace, preheated at 350°C for 20 minutes at a heating rate of 10°C / min, then heated to 1050°C and sintered for 10 minutes. After sintering, the power is turned off and the ball is naturally cooled to room temperature to obtain the finished sludge anaerobic digestion residue-based expanded clay.

[0053] Comparative Example 1

[0054] The present embodiment provides a method for preparing ceramsite using anaerobic digestion residue of sludge. Specifically, the method comprises the following raw materials in weight percentage: 42.5% anaerobic digestion residue of sludge, 42.5% fly ash, and 15% clay.

[0055] This embodiment also provides a method for preparing ceramsite using sludge anaerobic digestion residue, comprising the following steps:

[0056] S1 Raw material drying: Put the anaerobic digestion residue of sludge with a mass moisture content of 78% into a blast drying oven and dry the moisture at a temperature of 105°C to make its mass moisture content less than 5%;

[0057] S2 raw material grinding: putting the anaerobic digestion residue of sludge dried in step S1 into a grinder for grinding, passing the ground anaerobic digestion residue powder through a 100-mesh sieve, and taking the sieve residue and saving it for later use;

[0058] S3 weighing, stirring and mixing: weighing a certain amount of the sludge anaerobic digestion residue powder, fly ash powder and clay powder dried in step S2 according to the mass percentage, putting the weighed three raw material powders into the same container, and mixing them under the action of a fast mixer for later use;

[0059] S4 granulation and balling: add appropriate amount of water to the raw material powder mixed in step S3 to make its moisture content 25%, use a granulator to make balls, and obtain raw material balls with a particle size of 6 mm;

[0060] S5: drying the raw balls: placing the raw balls prepared in step S4 into a blast drying oven and drying them at 105°C for 6 hours;

[0061] S6 high temperature sintering: put the raw material balls dried in step S5 into a box-type resistance furnace, preheat at 350°C for 25 minutes at a heating rate of 10°C / min, then heat to 1050°C and sinter for 10 minutes. After sintering, turn off the power and cool naturally to room temperature to obtain finished sludge anaerobic digestion residue-based expanded clay.

[0062] Comparative Example 2

[0063] The present embodiment provides a method for preparing ceramsite using sludge anaerobic digestion residue, which specifically comprises the following raw materials in weight percentage: 54% sludge anaerobic digestion residue, 36% fly ash, and 10% clay.

[0064] This embodiment also provides a method for preparing ceramsite using sludge anaerobic digestion residue, comprising the following steps:

[0065] S1 Raw material drying: Put the anaerobic digestion residue of sludge with a mass moisture content of 78% into a blast drying oven and dry the moisture at a temperature of 105°C to make its mass moisture content less than 5%;

[0066] S2 raw material grinding: putting the anaerobic digestion residue of sludge dried in step S1 into a grinder for grinding, passing the ground anaerobic digestion residue powder through a 100-mesh sieve, and taking the sieve residue and saving it for later use;

[0067] S3 weighing, stirring and mixing: weighing a certain amount of the sludge anaerobic digestion residue powder, fly ash powder and clay powder dried in step S2 according to the mass percentage, putting the weighed three raw material powders into the same container, and mixing them under the action of a fast mixer for later use;

[0068] S4 granulation and balling: add appropriate amount of water to the raw material powder mixed in step S3 to make its moisture content 30%, use a granulator to make balls, and obtain raw material balls with a particle size of 6 mm;

[0069] S5: drying the raw material balls: placing the raw material balls prepared in step S4 into a blast drying oven and drying them at 105°C for 8 hours;

[0070] S6 high temperature sintering: put the raw material balls dried in step S5 into a box-type resistance furnace, preheat at 350°C for 25 minutes at a heating rate of 10°C / min, then heat to 1050°C and sinter for 10 minutes. After sintering, turn off the power and cool naturally to room temperature to obtain finished sludge anaerobic digestion residue-based expanded clay.

[0071] The raw materials used in the anaerobic digestion residue-based ceramsite prepared in the above Examples 1-3 and Comparative Examples 1-2 are shown in Table 1 below:

[0072] Table 1 Percentage content of raw material formula of ceramsite trial product fired from anaerobic digestion residue of sludge

[0073] raw material Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Sewage sludge anaerobic digestion residue 45% 48% 51% 42.5% 54% Fly ash 30% 32% 34% 42.5% 36% Clay 25% 20% 15% 15% 10%

[0074] The density, apparent density, porosity, water absorption rate and abrasion rate of the anaerobic digestion residue-based ceramsite prepared in the above Examples 1-3 and Comparative Examples 1-2 were tested according to the Chinese industry standard CJ / T 299-2008.

[0075] The test results are shown in Table 2 below:

[0076] Table 2 Test results of various performance parameters of anaerobic digestion residue-based expanded clay pellets.

[0077] Test Results Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 <![CDATA[Density g / cm 3 > 2.226 2.224 2.250 2.177 2.271 <![CDATA[Apparent density g / cm 3 > 1.634 1.612 1.556 1.586 1.548 Porosity% 56.76 56.82 58 56.95 58.96 Water absorption % 47.88 49.85 50.08 47.35 54.64 Wear rate % 3.92 4.09 4.37 10.42 7.55

[0078] It can be seen from Table 2 that when the percentage of anaerobic digestion residues in the anaerobic digestion residue-based ceramsite raw material formula is less than 45% and the percentage of anaerobic digestion residues is greater than 51%, the wear rate of the prepared anaerobic digestion residue-based ceramsite is higher than the limit required by the Chinese industry standard CJ / T 299-2008. Other performance indicators are far better than the ceramsite prepared by patent CN 115322007 A and patent CN 113880477 A using other raw materials. The SiO2 and Al2O3 contents in the anaerobic digestion residue of sludge are relatively low, while the content of metal oxide solvents is relatively high. In Comparative Example 2, the amount of anaerobic digestion residue of sludge added is relatively large, and the SiO2 and Al2O3 contents in the overall raw material formula are relatively low. The skeleton formed by the eutectic of SiO2 and Al2O3 is relatively small, resulting in a relatively large wear rate of the sintered ceramsite. However, the content of metal oxide solvents is relatively high, which reduces the eutectic temperature of the mixture, increases the liquid phase content, reduces the crystal viscosity, and causes a large amount of gas to escape. The pores formed are quickly filled with a low-viscosity liquid phase, increasing the proportion of the solid part and the blocked pore part of the ceramsite, thereby increasing the density and apparent density of the anaerobic digestion residue-based ceramsite as the amount of clay added increases, while the porosity and water absorption rate decrease. In Comparative Example 1, the amount of sludge anaerobic digestion residue added is relatively small, the content of SiO2 and Al2O3 in the overall raw material formula is relatively high, and the content of metal oxide solvent is relatively low, which increases the eutectic temperature of the mixture. At a certain temperature, the skeleton strength formed by the eutectic of SiO2 and Al2O3 is relatively low, so the wear rate of expanded clay is relatively large.

[0079] Application Example 1

[0080] The ceramsite prepared in Example 3 was used as an ozone catalyst in the deep treatment process of phenol-containing wastewater.

[0081] This application example uses phenol solution to replace phenol-containing wastewater, and the COD is about 300 mg / L.

[0082] The method of using sludge anaerobic digestion residue-based ceramsite as an ozone catalyst, the specific steps are as follows:

[0083] This application example designs three different O3 catalytic oxidation systems for organic pollutants, namely, a single O3 system, a sludge anaerobic digestion residue-based ceramsite + air system, and a sludge anaerobic digestion residue-based ceramsite + O3 system.

[0084] S1 O3 system alone: ​​Take a 100ml glass reagent bottle, insert the glass tube equipped with an aeration head to the bottom, add 100ml phenol solution into the reagent bottle, Ph=6, gas addition rate is 1L / min, ozone concentration in the gas is 5mg / L, take samples at 5min, 10min, 15min, 20min, 25min, 30min, 40min, 50min, 60min of reaction time to determine the organic matter concentration;

[0085] S2 sludge anaerobic digestion residue-based ceramsite + air system: take a 100ml glass reagent bottle, insert a glass tube equipped with an aeration head to the bottom of the glass reagent bottle, add 10g of sludge anaerobic digestion residue-based ceramsite prepared in Example 3 into the reagent bottle, add 100ml of phenol solution into the reagent bottle, Ph=6, gas addition rate is 1L / min, ozone concentration in the gas is 0mg / L, and samples are taken at reaction time of 5min, 10min, 15min, 20min, 25min, 30min, 40min, 50min, 60min to determine the organic matter concentration;

[0086] S3 sludge anaerobic digestion residue-based ceramsite + O3 system: take a 100ml glass reagent bottle, insert a glass tube equipped with an aeration head to the bottom of the glass reagent bottle, add 10g of sludge anaerobic digestion residue-based ceramsite prepared in Example 3 into the reagent bottle, add 100ml of phenol solution into the reagent bottle, Ph=6, gas addition rate is 1L / min, ozone concentration in the gas is 5mg / L, take samples at reaction time of 5min, 10min, 15min, 20min, 25min, 30min, 40min, 50min, 60min to determine the organic matter concentration;

[0087] In this application example, the anaerobic digestion residue-based ceramsite prepared in Example 3 is used as an ozone catalyst to treat phenol-containing wastewater. The treatment effect is shown in Table 3.

[0088] Table 3 Comparison of the application effects of sludge anaerobic digestion residue-based ceramsite as ozone catalyst

[0089]

[0090] In this application example, it can be seen from Table 3 that the anaerobic digestion residue-based ceramsite + air system has a low removal efficiency for organic matter in sewage and cannot remove organic matter in sewage. The removal rate of organic matter in the pure O3 system after 60 minutes of reaction is 81.92%; while the removal rate of organic matter in sewage in the anaerobic digestion residue-based ceramsite + O3 system reaches more than 95% after 20 minutes of reaction. At the same time, it is 28.1% higher than the pure O3 system. It can be seen that the use of anaerobic digestion residue-based ceramsite as an ozone catalyst significantly improves the catalytic oxidation effect of O3.

[0091] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An application of ceramsite as an ozone catalyst, characterized in that: According to weight percentage, the raw material composition of the ceramsite is 45%-51% of anaerobic digestion residue of sludge, 30%-34% of fly ash, and 15%-25% of clay; The ceramsite is prepared by using the residue of anaerobic digestion of sludge, and the steps are as follows: S1 Raw material drying: Put the anaerobic digestion residue of sludge into a blast drying oven and dry it at a temperature of 105°C to make its moisture content less than 5%; S2 raw material grinding: putting the anaerobic digestion residue of sludge dried in step S1 into a grinder for grinding, passing the ground anaerobic digestion residue powder through a 100-mesh sieve, and taking the sieve residue and saving it for later use; S3 weighing, stirring and mixing: weighing a certain amount of sludge anaerobic digestion residue powder, fly ash powder and clay powder according to mass percentage, putting the weighed three raw material powders into the same container, and mixing them under the action of a fast mixer for later use; S4 granulation and balling: adding water to the raw material powder mixed in step S3 until the moisture content is 20%-35%, using a granulator to make balls to obtain raw material balls with a particle size of 6 mm; S5: drying the raw balls: placing the raw balls prepared in step S4 into a blast drying oven and drying them at 105°C for 6 hours; S6 high temperature sintering: the raw material balls dried in step S5 are placed in a box-type resistance furnace, preheated at 350°C for 25 minutes, then heated to 1050°C, and sintered for 10 minutes. After the sintering is completed, the power is turned off and the temperature is naturally cooled to room temperature to obtain sludge anaerobic digestion residue-based ceramsite; The ceramsite is used as an ozone catalyst for deep treatment of phenol-containing wastewater; The sludge is coagulated sludge containing iron.

2. The use of ceramsite as an ozone catalyst according to claim 1, characterized in that: According to weight percentage, the raw material composition of the ceramsite is: 51% of sludge anaerobic digestion residue, 34% of fly ash, and 15% of clay.

3. The use of ceramsite as an ozone catalyst according to claim 1 or 2, characterized in that: The fly ash powder is fly ash that has been dried, manually ground, and then sieved through a 100-mesh sieve to obtain the undersize.

4. The use of ceramsite as an ozone catalyst according to claim 1 or 2, characterized in that: The clay powder is the undersize obtained by drying the clay, grinding it manually and using a 100-mesh sieve.