Aluminate-based red luminescent material and preparation method and application thereof
Prepared by sol-gel method of aluminate-based red-luminescent material, the crystal field perturbation of Eu3+ is enhanced by B3+ doping, and the problem of low excitation efficiency of europium ion activators in the near-ultraviolet-blue light band in the prior art is solved, and the problem of low excitation efficiency of europium ion activators in the near-ultraviolet-blue light band is realized. High-efficiency red light emission, suitable for white LED applications, and has simple process, environmental protection and low energy consumption.
Patent Information
- Application Number
- CN202310649399.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-06-02
AI Technical Summary
The existing europium ion activated phosphor has low excitation efficiency in the near-ultraviolet-blue light band and is difficult to match the emission band of LED illumination, which limits the application of white LEDs.
The chemical formula of the aluminate-based red-luminescent material is Sr0.5Ba4.5Al2O8:xEu3+,yB3+, which is prepared by sol-gel method. The crystal field disturbance of Eu3+ is enhanced by B3+ doping, and the efficient 5D0→7F2 electric dipole luminescence transition is achieved. , emits red light with a wavelength of 615 nanometers.
It achieves efficient red light emission in the near-ultraviolet and blue light bands, with pure chromaticity and high luminous efficiency, which is suitable for the needs of white LEDs. It also has a simple preparation process, low cost, environmentally friendly, low sintering temperature, and saves energy consumption.
Smart Images

Figure CN116875303B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic luminescent materials, and in particular relates to an aluminate-based red luminescent material and a preparation method and application thereof. Background Art
[0002] Rare earth ions play an important role as activators in luminescent display materials. Rare earth ions have a special electronic configuration and can emit wide-band fluorescence in the ultraviolet-visible-infrared range. 3+ ) is the most important red luminescent activator. Europium ions can be excited by ultraviolet, near-ultraviolet, or blue light bands and emit a linear red luminescence spectrum with concentrated energy and pure redness. The fluorescent pink activated by europium ions has high luminescence efficiency and good temperature stability. However, the absorption resonance efficiency of europium ions themselves in the ultraviolet-visible light wavelength range is very low, and its excitation generally comes from two parts. The first is Eu 3+ -
[0003] O 2- The charge transfer band between the two is generally located in the ultraviolet band, which is suitable for mercury lamp lighting, but is obviously not compatible with the emission of near-ultraviolet-blue LED semiconductor chips used in LED lighting. The second excitation source is from Eu 3+ The ff absorption transitions of the phosphors are located in the near-ultraviolet (380-400 nanometers) and blue (450-460 nanometers) bands, which are very compatible with the emission of commercial ultraviolet-blue LED semiconductor chips. As phosphors, they are particularly suitable for white-light LED lighting. Therefore, it is very important to develop luminescent materials with good excitation in the near-ultraviolet-blue band for white-light lighting. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art, and provides an aluminate-based red luminescent material and a preparation method and application thereof.
[0005] In one aspect of the present invention, an aluminate-based red luminescent material is provided, wherein the chemical formula of the aluminate-based red luminescent material is Sr 0.5 Ba 4.5 Al2O8:xEu 3+ ,yB 3+ ; where x is Eu 3+ Replace Ba 2+ The number of moles of B 3+ Replace Al 3+ The number of moles, and 0.0225≤x≤0.36, 0≤y≤0.1.
[0006] Optionally, the aluminate-based red luminescent material emits red light with a wavelength of 615 nanometers under excitation in the near-ultraviolet and blue light bands.
[0007] Another aspect of the present invention provides a method for preparing the aluminate-based red luminescent material as described above, the method comprising:
[0008] Sr 2+ Compounds containing Ba 2+ Compounds containing Al 3+ Compounds containing B 3+ Compounds containing Eu 3+ The compound is used as the raw material, according to the chemical formula Sr 0.5 Ba 4.5 Al2O8:xEu 3+ ,yB 3+ Weigh each raw material according to the stoichiometric ratio of the corresponding elements in (0.0225≤x≤0.36, 0≤y≤0.1);
[0009] Dissolve each raw material in a dilute nitric acid solution or deionized water to form a transparent solution after complete dissolution, add citric acid or oxalic acid as a complexing agent to each transparent solution, and the amount of the complexing agent added is 1.5 to 2.0 times the molar number of cations in each transparent solution; then stir at a temperature of 70° C. to 100° C. for 0.5 to 1 hour, and then slowly mix the various solutions together to obtain a transparent mixed solution;
[0010] Adding ethylene glycol as a polymerization agent to the mixed solution at 70° C. to 90° C. with continuous stirring to obtain a viscous sol, and then drying the sol at 110-150° C. for 10-15 hours to obtain a xerogel;
[0011] calcining the dry gel at 400° C.-500° C. for 1-5 hours, grinding, and obtaining a precursor mixture;
[0012] The precursor mixture is calcined at 1000° C.-1200° C. for 1-10 hours to obtain an aluminate-based red luminescent material.
[0013] Optionally, the Ba-containing 2+ The compound is Ba-containing 2+ Oxide, containing Ba 2+ Hydroxide containing Ba 2+ One or more salts of
[0014] Optionally, the Sr-containing 2+ The compound is Sr-containing 2+ Oxides, containing Sr 2+ Hydroxide, containing Sr 2+One or more salts of
[0015] Optionally, the Eu-containing 3+ The compound is Eu 3+ Oxide, containing Eu 3+ Salts and Eu 3+ One or more rare earth organic complexes.
[0016] Optionally, the B 3+ The compound is boric acid and / or boron trioxide.
[0017] Optionally, the Al-containing 3+ The compound is any one of aluminum nitrate, aluminum oxide, and aluminum hydroxide.
[0018] Optionally, the precursor mixture is calcined at a temperature of 1050°C-1150°C.
[0019] Another aspect of the present invention provides an application of an aluminate-based red luminescent material, wherein the aluminate-based red luminescent material described above is combined with blue and green phosphors to coat and encapsulate an InGaN diode to prepare a white light LED lighting device.
[0020] The present invention provides an aluminate-based red luminescent material and a preparation method and application thereof, which have the following beneficial effects compared with the prior art solutions:
[0021] First, the luminescent material of the present invention has the following advantages in terms of the structure of the matrix: First, the matrix lattice is a three-dimensional network composed of Al-O tetrahedrons, which has high rigidity and strength. Therefore, the luminescent thermal stability of the phosphor is good, it can withstand high-density excitation, and has good physical-chemical stability; Second, B 3+ In Al 3+ Lattice site doping realizes Eu 3+ The strong disturbance of the crystal field is conducive to the full splitting of its energy levels, especially for Eu 3+ of 5 D0
[0022] → 7 The electric dipole luminescence transition of F2 is used to obtain a phosphor with high crystallinity, fine particles, pure chromaticity and high luminescence efficiency;
[0023] Second, the advantages of the luminescent material of the present invention in terms of application performance are as follows: it can be excited by ultraviolet-near ultraviolet and blue light bands, and the luminescent spectrum is located at 615 nanometers, which comes from 5 D0→ 7 The sharp luminescence peak of F2 transition has good luminescence efficiency and pure red chromaticity;
[0024] Third, the advantages of the method for preparing the luminescent material of the present invention are as follows: the aluminate-based red luminescent material is synthesized by a simple and easy sol-gel method, the preparation process is simple, the raw materials are easily available, the cost is low, there is no pollution, no waste gas or waste liquid emissions, it is environmentally friendly, and easy to produce; in addition, the final sintering temperature is low, and the matrix can be well crystallized in pure phase at 1050°C-1150°C, saving energy. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 1 is a flowchart of a method for preparing an aluminate-based red luminescent material according to an embodiment of the present invention;
[0026] Figure 2 The XRD diffraction patterns of the samples prepared in Examples 1, 2, 3 and 4 of the present invention are compared with the X-ray diffraction standard card PDF#26-0224 (Ba5Al2O8);
[0027] Figure 3 This is a scanning electron microscope image of the sample prepared in Example 1 of the present invention;
[0028] Figure 4 The luminescence spectrum of the sample prepared in Example 1 of the present invention;
[0029] Figure 5 is the excitation spectrum of the sample prepared in Example 1 of the present invention;
[0030] Figure 6 is the luminescence decay curve of the sample prepared in Example 1 of the present invention;
[0031] Figure 7 The luminescence spectrum of the sample prepared in Example 2 of the present invention;
[0032] Figure 8 Excitation spectrum of the sample prepared in Example 2 of the present invention;
[0033] Fig. 9 is the luminescence decay curve of the sample prepared in Example 2 of the present invention;
[0034] Fig.10 The luminescence spectrum of the sample obtained in Example 3 of the present invention is
[0035] Fig.11 Excitation spectrum of the sample prepared in Example 3 of the present invention;
[0036] Fig.12 This is the luminescence decay curve of the sample prepared in Example 3 of the present invention;
[0037] Fig.13 The luminescence spectrum of the sample prepared in Example 4 of the present invention;
[0038] Fig.14 Excitation spectrum of the sample prepared in Example 4 of the present invention;
[0039] Fig.15 This is the luminescence attenuation curve of the sample prepared in Example 4 of the present invention. DETAILED DESCRIPTION
[0040] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the described embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative work are within the scope of protection of the present invention.
[0041] In one aspect of the present invention, an aluminate-based red luminescent material is provided, wherein the matrix of the aluminate-based red luminescent material is an aluminate oxide, and the activator is a trivalent europium ion (Eu 3+ ), whose chemical formula is Sr 0.5 Ba 4.5 Al2O8:xEu 3+ ,yB 3+ ; where x is a europium ion (Eu 3+ ) replaces the barium ion (Ba 2+ ) molar number, y is the number of boron ions (B 3+ ) replaces aluminum ions (Al 3+ ), and 0.0225≤x≤0.36, 0≤y≤0.1.
[0042] In this embodiment, the structural advantages of the aluminate-based red luminescent material are: first, the matrix lattice is a three-dimensional network composed of Al-O tetrahedrons, which has high rigidity, so the luminescent thermal stability of the phosphor is good, it can withstand high-density excitation, and has good physical-chemical stability; second, B 3+ In Al 3+ Lattice site doping realizes Eu 3+ The strong disturbance of the crystal field is conducive to the full splitting of its energy levels, especially for Eu 3+ of 5 D0→ 7 The electric dipole luminescence transition of F2 is used to obtain a phosphor with pure chromaticity and high luminescence efficiency, which can be used as a light conversion material for near-ultraviolet LED chips and blue light LED chips to achieve red light emission.
[0043] Furthermore, the luminescent material of this embodiment can be excited by near-ultraviolet and blue light bands and emits a sharp red light spectrum with a main peak at 615 nanometers, that is, the luminescent spectrum shows a red light at 615 nanometers, which is derived from 5 D0→ 7The F2 transition has a sharp luminescence peak. The luminescent material has good luminescence efficiency, pure red chromaticity, and no afterglow phenomenon, which is suitable for lighting needs.
[0044] like Figure 1 As shown, another aspect of the present invention provides a method S100 for preparing the aluminate-based red luminescent material described above, comprising the following steps S110 to S150:
[0045] S110, containing strontium ions (Sr 2+ ) compounds, barium ions (Ba 2+ ) compounds, aluminum ions (Al 3+ ) compounds, boron ions (B 3+ ) compounds, europium ions (Eu 3+ ) as raw materials, according to the chemical formula Sr 0.5 Ba 4.5 Al2O8:xEu 3+ ,yB 3+ Weigh each raw material according to the stoichiometric ratio of the corresponding elements in (0.0225≤x≤0.36, 0≤y≤0.1).
[0046] Specifically, in step S110, the barium ion (Ba 2+ ) is Ba 2+ The present invention can be one or a combination of two or more of oxides, hydroxides, various salts (such as carbonates, nitrates, oxalates, sulfates, halides). For example, barium nitrate Ba(NO3)2 can be preferably used.
[0047] Furthermore, in step S110, the strontium ion (Sr 2+ ) is Sr 2+ The present invention can be one or a combination of two or more of oxides, hydroxides, various salts (such as carbonates, nitrates, oxalates, sulfates, halides). For example, strontium nitrate Sr(NO3)2 can be preferred.
[0048] Furthermore, in step S110, the europium ion (Eu 3+ ) is Eu 3+ The present invention can be one of oxides, salts (such as nitrates, oxalates and sulfates) and rare earth organic complexes or a combination thereof. For example, europium nitrate Eu(NO3)3·6H2O can be preferred.
[0049] Furthermore, in step S110, the boron ion (B 3+ ) is boric acid, boron trioxide or a combination thereof. For example, boric acid H3BO3 may be preferred.
[0050] Furthermore, in step S110, the aluminum ion (Al3+ ) is one of aluminum nitrate, aluminum oxide, and aluminum hydroxide. For example, aluminum nitrate Al(NO3)3·9H2O is preferred.
[0051] S120, dissolving the raw materials weighed in step S110 in dilute nitric acid solution or deionized water respectively, and preparing respective transparent solutions after complete dissolution, adding citric acid or oxalic acid as a complexing agent to each solution, and the amount added is 1.5 to 2.0 times the molar number of cations in the respective solution; then stirring at a temperature of 70°C to 100°C for 0.5 to 1 hour, and then slowly mixing the various solutions together to obtain a transparent mixed solution.
[0052] S130, adding an appropriate amount of ethylene glycol as a polymerization agent to the mixed solution obtained in step S120 at 70° C. to 90° C. with continuous stirring to obtain a viscous sol, and then placing the sol in an oven and drying it at 110-150° C. for 10-15 hours to obtain a xerogel;
[0053] S140, calcining the dry gel at 400° C.-500° C. for 1-5 hours, and grinding appropriately to obtain a precursor mixture;
[0054] S150, calcining the precursor mixture obtained in step S140 at 1000°C-1200°C for 1-10 hours to obtain a final white powder product, which is an aluminate-based red luminescent material.
[0055] In step S150, the calcination temperature may preferably be 1050°C-1150°C.
[0056] In this embodiment, aluminate-based red luminescent materials are prepared by a simple and easy chemical sol-gel synthesis method. The preparation process is simple, pollution-free, and has no waste gas or waste liquid emissions, and is easy to produce. Moreover, during the preparation process, the sintering temperature of the luminescent material is low, and the matrix can be well crystallized in pure phase at 1050-1150°C, that is, a pure phase product can be obtained at a lower synthesis temperature, saving energy.
[0057] Another aspect of the present invention provides an application of an aluminate-based red luminescent material. The aluminate-based red luminescent material described above can be combined with an appropriate amount of blue and green phosphors, coated and packaged outside an InGaN diode to prepare a white LED lighting device.
[0058] It should be noted that the luminescent material according to this embodiment can be excited by ultraviolet-near ultraviolet and blue light bands, and the luminescent spectrum is located at 615 nanometers, which comes from 5 D0→ 7The sharp luminescence peak of F2 transition, good luminescence efficiency, pure red chromaticity, and no afterglow phenomenon can be used to combine the aluminate-based red luminescent material with appropriate amounts of blue and green phosphors, coat and encapsulate it outside the InGaN diode to prepare a white light LED lighting device.
[0059] The preparation method and performance of aluminate-based red luminescent materials will be further described below in conjunction with several specific examples:
[0060] Example 1
[0061] The method for preparing the aluminate-based red luminescent material of this example comprises the following steps:
[0062] S1, according to the chemical formula Sr 0.5 Ba 4.5 Al2O8:0.0225Eu 3+ The corresponding elements in the chemical stoichiometric ratio are weighed: strontium nitrate Sr(NO3)2: 0.794 g, barium nitrate Ba(NO3)2: 8.776 g, europium nitrate Eu(NO3)3·6H2O: 0.075 g, aluminum nitrate Al(NO3)3·9H2O: 5.627 g;
[0063] S2, dissolving the raw materials weighed in step S1 in dilute nitric acid solution respectively, and adding 0.506 g of oxalic acid to the strontium nitrate solution, 4.535 g of oxalic acid to the barium nitrate solution, 0.023 g of oxalic acid to the europium nitrate solution, and 2.026 g of oxalic acid to the aluminum nitrate solution; stirring each of the above solutions at 70° C. for 1 hour, and then slowly mixing the various solutions together to obtain a transparent mixed solution;
[0064] S3, adding an appropriate amount of ethylene glycol as a polymerization agent to the mixed solution obtained in step S2 at 90° C. with continuous stirring to obtain a viscous sol, and then placing the sol in an oven and drying it at 110° C. for 15 hours to obtain a xerogel;
[0065] S4, calcining the xerogel obtained in step S3 at 500° C. for 1 hour, and grinding appropriately to obtain a precursor mixture;
[0066] S5. calcining the precursor mixture obtained in step S4 at 1200° C. for 1 hour to obtain a white powder, namely, an aluminate-based red luminescent material.
[0067] Further, see Appendix Figure 2 , the comparison results of the X-ray powder diffraction pattern of the sample obtained in Example 1 and the standard card PDF#26-0224 are given. The pattern of the sample is completely consistent with the standard card, indicating that the obtained substance is a pure phase.
[0068] For further information, see Appendix Figure 3 , a scanning electron microscope image of the sample obtained in Example 1 is given, and the sample presents spherical particles with uniform size and a particle size of 400-500 nanometers, indicating that the luminescent material particles prepared in this example are fine.
[0069] For further information, see Appendix Figure 4 , the luminescence spectrum of the sample obtained in Example 1 is given, and the main luminescence center is a sharp red luminescence peak of 615 nanometers with pure chromaticity.
[0070] For further information, see Appendix Figure 5 , the excitation spectrum of the sample obtained in Example 1 is given. It can be seen that the excitation source of the red light emission of the material comes from the ultraviolet, near-ultraviolet and blue light bands, which matches the commercial near-ultraviolet and blue light LEDs.
[0071] For further information, see Appendix Figure 6 , the luminescence decay curve of the sample obtained in Example 1 is given, and it can be calculated that the decay time of the red phosphor is 1.52 milliseconds, and the luminescence will not produce afterglow phenomenon, which is suitable for lighting needs.
[0072] Example 2
[0073] The method for preparing the aluminate-based red luminescent material of this example comprises the following steps:
[0074] S1, according to the chemical formula Sr 0.5 Ba 4.5 Al2O8:0.135Eu 3+ ,0.04B 3+ The corresponding elements in the chemical stoichiometric ratio are weighed: strontium nitrate Sr(NO3)2: 0.688 g, barium nitrate Ba(NO3)2: 7.415 g, europium nitrate Eu(NO3)3·6H2O: 0.391 g, aluminum nitrate Al(NO3)3·9H2O: 4.779 g, boric acid H3BO3: 0.016 g;
[0075] S2, dissolving the raw materials weighed in step S1 in dilute nitric acid solution respectively, and adding 0.585 g of oxalic acid to the strontium nitrate solution, 5.109 g of oxalic acid to the barium nitrate solution, 0.158 g of oxalic acid to the europium nitrate solution, 2.294 g of oxalic acid to the aluminum nitrate solution, and 0.047 g of oxalic acid to the boric acid solution; stirring each of the above solutions at 100° C. for 0.5 hour, and then slowly mixing the various solutions together to obtain a transparent mixed solution;
[0076] S3, adding an appropriate amount of ethylene glycol as a polymerization agent to the mixed solution obtained in step S2 at 70° C. with continuous stirring to obtain a viscous sol, and then placing the sol in an oven and drying it at 150° C. for 10 hours to obtain a xerogel;
[0077] S4, calcining the xerogel obtained in step S3 at 400° C. for 5 hours, and grinding appropriately to obtain a precursor mixture;
[0078] S5. calcining the precursor mixture obtained in step S4 at 1000° C. for 10 hours to obtain a white powder, namely, an aluminate-based red luminescent material.
[0079] Further, see Appendix Figure 2 , the comparison results of the X-ray powder diffraction pattern of the sample obtained in Example 2 and the standard card PDF#26-0224 are given. The pattern of the sample is completely consistent with the standard card, indicating that the obtained substance is a pure phase.
[0080] For further information, see Appendix Figure 7 , the luminescence spectrum of the sample obtained in Example 2 is given, and the main luminescence center is a sharp red luminescence peak of 615 nanometers with pure chromaticity.
[0081] For further information, see Appendix Figure 8 , which is the excitation spectrum of the sample obtained in Example 2, it can be seen that the excitation source of the red light emission of this material comes from the ultraviolet, near-ultraviolet and blue light bands, which matches the commercial near-ultraviolet and blue light LEDs.
[0082] For further information, see Appendix Fig. 9 , the luminescence decay curve of the sample obtained in Example 2 is given, and it can be calculated that the decay time of the red phosphor is 1.31 milliseconds, and the luminescence will not produce afterglow phenomenon, which is suitable for lighting needs.
[0083] Example 3
[0084] The method for preparing the aluminate-based red luminescent material of this example comprises the following steps:
[0085] S1, according to the chemical formula Sr 0.5 Ba 4.5 Al2O8:0.27Eu 3+ ,0.06B 3+ The corresponding elements in the chemical stoichiometric ratio are weighed: strontium nitrate Sr(NO3)2: 0.794 g, barium nitrate Ba(NO3)2: 8.291 g, europium nitrate Eu(NO3)3·6H2O: 0.903 g, aluminum nitrate Al(NO3)3·9H2O: 5.458 g, boric acid H3BO3: 0.028 g;
[0086] S2, dissolving the raw materials weighed in step S1 in dilute nitric acid solution respectively, and adding 1.081 g of citric acid to the strontium nitrate solution, 9.143 g of citric acid to the barium nitrate solution, 0.584 g of citric acid to the europium nitrate solution, 4.193 g of citric acid to the aluminum nitrate solution, and 0.13 g of citric acid to the boric acid solution; stirring the above solutions at 90° C. for 0.5 hour respectively, and then slowly mixing the various solutions together to obtain a transparent mixed solution;
[0087] S3, adding an appropriate amount of ethylene glycol as a polymerization agent to the mixed solution obtained in step S2 at 85° C. with continuous stirring to obtain a viscous sol, and then placing the sol in an oven and drying it at 150° C. for 6 hours to obtain a xerogel;
[0088] S4, calcining the xerogel obtained in step S3 at 450° C. for 4 hours, and grinding appropriately to obtain a precursor mixture;
[0089] S5. calcining the precursor mixture obtained in step S4 at 1100° C. for 8 hours to obtain a white powder, namely, an aluminate-based red luminescent material.
[0090] Further, see Appendix Figure 2 , the comparison results of the X-ray powder diffraction pattern of the sample obtained in Example 3 and the standard card PDF#26-0224 are given. The pattern of the sample is completely consistent with the standard card, indicating that the obtained substance is a pure phase.
[0091] For further information, see Appendix Fig.10 , the luminescence spectrum of the sample obtained in Example 3 is given, and the main luminescence center is a sharp red luminescence peak of 615 nanometers with pure chromaticity.
[0092] For further information, see Appendix Fig.11 , the excitation spectrum of the sample obtained in Example 3 is given. It can be seen that the excitation source of the red light emission of the material comes from the ultraviolet, near-ultraviolet and blue light bands, which matches the commercial near-ultraviolet and blue light LEDs.
[0093] For further information, see Appendix Fig.12 , the luminescence decay curve of the sample obtained in Example 3 is given, and it can be calculated that the decay time of the red phosphor is 1.05 milliseconds, and the luminescence will not produce afterglow phenomenon, which is suitable for lighting needs.
[0094] Example 4
[0095] The method for preparing the aluminate-based red luminescent material of this example comprises the following steps:
[0096] S1, according to the chemical formula Sr 0.5 Ba 4.5Al2O8:0.36Eu 3+ ,0.1B 3+ The corresponding elements in the chemical stoichiometric ratio are weighed: strontium nitrate Sr(NO3)2: 0.582 g, barium nitrate Ba(NO3)2: 5.951 g, europium nitrate Eu(NO3)3·6H2O: 0.883 g, aluminum nitrate Al(NO3)3·9H2O: 3.92 g, boric acid H3BO3: 0.034 g;
[0097] S2, dissolving the raw materials weighed in step S1 in dilute nitric acid solution respectively, and adding 1.057 g of citric acid to the strontium nitrate solution, 8.75 g of citric acid to the barium nitrate solution, 0.761 g of citric acid to the europium nitrate solution, 4.016 g of citric acid to the aluminum nitrate solution, and 0.211 g of citric acid to the boric acid solution; stirring each of the above solutions at 90° C. for 1 hour, and then slowly mixing the various solutions together to obtain a transparent mixed solution;
[0098] S3, adding an appropriate amount of ethylene glycol as a polymerization agent to the mixed solution obtained in step S2 at 90° C. with continuous stirring to obtain a viscous sol, and then placing the sol in an oven and drying it at 150° C. for 6 hours to obtain a xerogel;
[0099] S4, calcining the xerogel obtained in step S3 at 450° C. for 4 hours, and grinding appropriately to obtain a precursor mixture;
[0100] S5. calcining the precursor mixture obtained in step S4 at 1100° C. for 5 hours to obtain a white powder, which is an aluminate-based red luminescent material.
[0101] Further, see Appendix Figure 2 , the comparison results of the X-ray powder diffraction pattern of the sample obtained in Example 4 and the standard card PDF#26-0224 are given. The pattern of the sample is completely consistent with the standard card, indicating that the obtained substance is a pure phase.
[0102] For further information, see Appendix Fig.13 , the luminescence spectrum of the sample obtained in Example 4 is given, and the main luminescence center is a sharp red luminescence peak of 615 nanometers with pure chromaticity.
[0103] For further information, see Appendix Fig.14 , the excitation spectrum of the sample obtained in Example 4 is given. It can be seen that the excitation source of the red light emission of the material comes from the ultraviolet, near-ultraviolet and blue light bands, which matches the commercial near-ultraviolet and blue light LEDs.
[0104] For further information, see Appendix Fig.15, the luminescence decay curve of the sample obtained in Example 4 is given, and it can be calculated that the decay time of the red phosphor is 0.77 milliseconds, and the luminescence will not produce afterglow phenomenon, which is suitable for lighting needs.
[0105] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. An aluminate-based red luminescent material, It is characterized in that The chemical formula of the aluminate-based red luminescent material is Sr 0.5 Ba 4.5 Al 2 O 8 :xEu 3+ ,yB 3+ ; where x is Eu 3+ Replace Ba 2+ The number of moles of B 3+ Replace Al 3+ The molar number of, and 0.0225≤x≤0.36, 0≤y≤0.1; the aluminate-based red luminescent material emits red light with a wavelength of 615 nanometers under excitation in the ultraviolet, near-ultraviolet and blue light bands.
2. A method for preparing the aluminate-based red luminescent material according to claim 1, It is characterized in that The method comprises: Sr 2+ Compounds containing Ba 2+ Compounds containing Al 3+ Compounds containing B 3+ Compounds containing Eu 3+ The compound is used as the raw material, according to the chemical formula Sr 0.5 Ba 4.5 Al 2 O 8 :xEu 3+ ,yB 3+ , 0.0225≤x≤0.36, 0≤y≤0.1, weigh each raw material in the stoichiometric ratio of the corresponding elements; Dissolve each raw material in a dilute nitric acid solution or deionized water to form a transparent solution after complete dissolution, add citric acid or oxalic acid as a complexing agent to each transparent solution, and the amount of the complexing agent added is 1.5 to 2.0 times the molar number of cations in each transparent solution; then stir at a temperature of 70° C. to 100° C. for 0.5 to 1 hour, and then slowly mix the various solutions together to obtain a transparent mixed solution; Adding ethylene glycol as a polymerization agent to the mixed solution at 70° C. to 90° C. with continuous stirring to obtain a viscous sol, and then drying the sol at 110-150° C. for 10-15 hours to obtain a xerogel; calcining the dry gel at 400° C.-500° C. for 1-5 hours, grinding, and obtaining a precursor mixture; The precursor mixture is calcined at 1000° C.-1200° C. for 1-10 hours to obtain an aluminate-based red luminescent material.
3. The method according to claim 2, It is characterized in that The Ba-containing 2+ The compound is Ba-containing 2+ Oxide, containing Ba 2+ Hydroxide containing Ba 2+ One or more salts of 4. The method according to claim 2, It is characterized in that The Sr-containing 2+ The compound is Sr-containing 2+ Oxides, containing Sr 2+ Hydroxide, containing Sr 2+ One or more salts of 5. The method according to claim 2, It is characterized in that The Eu 3+ The compound is Eu 3+ Oxide, containing Eu 3+ Salts and Eu 3+ One or more rare earth organic complexes.
6. The method according to claim 2, It is characterized in that The B 3+ The compound is boric acid and / or boron trioxide.
7. The method according to claim 2, It is characterized in that The Al-containing 3+ The compound is any one of aluminum nitrate, aluminum oxide, and aluminum hydroxide.
8. The method according to claim 2, It is characterized in that The precursor mixture is calcined at a temperature of 1050°C-1150°C.
9. Application of an aluminate-based red luminescent material, It is characterized in that The aluminate-based red luminescent material described in claim 1 is used in combination with blue and green phosphors to prepare white light LED lighting devices.