Dual-phase nanocrystalline glass-ceramic materials with multi-spectral broadband tunable luminescence
By co-doping Mn2+ and Cr3+ ions in dual-phase glass ceramic materials, and by regulating the Ga2O3 content and doping concentration, Mn2+-Mn2+ dimers are formed, which solves the problem of constructing multi-color and ultra-broadband luminescent materials in the existing technology. The tunable multi-band composite broadband luminescence of 475-800nm is achieved, which enhances the spectrum coverage and luminous intensity.
Patent Information
- Application Number
- CN202310764805.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-06-27
AI Technical Summary
In the existing technology, Mn2+ or Cr3+ activated optical functional materials have the limitation of a single crystal when constructing multi-color and ultra-broadband luminescent materials, and the preparation of powder or single crystal materials is complex and expensive, and the crystallization process of dual-phase glass ceramics is complicated. , the related mechanism is not perfect, and it is difficult to meet the needs of multi-band broadband light sources.
Dual-phase glass-ceramic materials with Zn2SiO4 and ZnGa2O4 nanocrystals are used, and are co-doped with Mn2+ and Cr3+ ions. By regulating the Ga2O3 content and ion doping concentration, the formation of Mn2+-Mn2+ dimers is achieved, covering 475-800nm. Tunable multi-band composite broadband luminescence.
It has achieved tunable multi-band composite broadband luminescence covering 475-800nm in glass ceramic materials, increasing the number of luminescence bands and broadening the spectrum. By isolating Mn2+ and Cr3+ in local space, it effectively hinders luminescence quenching caused by energy transfer and improves luminescence. Controllability of intensity and band quantity.
Smart Images

Figure CN116891344B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field related to glass ceramics, and in particular relates to a dual-phase nanocrystalline glass ceramic material with multi-spectral broadband tunable luminescence. Background Art
[0002] Optical functional materials with tunable broadband luminescence have shown broad application prospects in cutting-edge technology fields such as temperature sensing, optical anti-counterfeiting, biomedicine, and plant light sources, and have become one of the current research hotspots in the field of materials science. Compared with rare earth ions, transition metal ions have the advantages of broadband emission, adjustable peak position, and long lifetime, and are considered to be ideal activation ions for obtaining broadband tunable luminescence. Among the many transition metal ions, Mn 2+ and Cr 3+ Due to the unique 3D 5 With 3D 3 The electronic configuration has adjustable broadband emission from the visible light region to the near-infrared region, and the excitation region covers the entire region from vacuum ultraviolet to yellow-green light. The luminescent materials activated by it usually have a wide luminescence range and excellent fluorescence properties. 2+ or Cr 3+ The activated luminescent matrix is mainly concentrated in powder, single crystal or glass ceramic. However, on the one hand, powder or single crystal materials have some disadvantages, such as: the packaging process of fluorescent powder materials is complicated, the growth conditions of crystal materials are harsh, the preparation cycle is long and the price is expensive, which is not conducive to the development of optoelectronic devices; on the other hand, although single-phase glass ceramics have the processability of glass materials and the excellent fluorescence properties of crystal materials, they can make up for the above shortcomings to a certain extent, but their crystals are single, and the luminescent environment provided for the activated ions is also relatively simple, which is more difficult to construct multi-color and ultra-wideband luminescent materials. Therefore, it is particularly important to develop matrix materials with a variety of crystal field environments.
[0003] In recent years, dual-phase glass-ceramics have attracted great attention from researchers. This material is composed of a glass phase and two different nanocrystals. It has the advantages of excellent mechanical properties and chemical stability of the glass phase and the fluorescence functions of the two different crystals. It can provide a variety of local luminescence environments for transition metal ions and is expected to meet the needs of multi-band broadband light sources. However, due to the complex crystallization process of dual-phase glass-ceramics and the imperfect related mechanisms, factors such as glass composition and ion doping concentration have a certain influence on the crystallization behavior and luminescence properties of dual-phase nanocrystals. It is necessary to further clarify the influence of these factors on the precipitation type of nanocrystals, ion occupation sites, and broadband spectra. Based on this, the Mn 2+ and Cr 3+ The preparation of co-doped dual-phase glass-ceramics and their tunable broadband luminescence are of great significance for expanding the application of transparent photonic glass materials in the field of multifunctional broadband light sources. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a dual-phase nanocrystalline glass-ceramic material with multi-spectral broadband tunable luminescence, wherein Zn2SiO4 nanocrystals and ZnGa2O4 nanocrystals are precipitated in the glass matrix and co-doped with transition metal ions Mn 2+ and Cr 3+ , achieving tunable multi-band composite broadband luminescence covering 475-800nm. And by high concentration doping of Mn 2+ The strategy can promote new luminescence centers (i.e., Mn 2+ -Mn 2+ dimer), realizing the single Mn 2+ To Mn 2+ -Mn 2+ The adjustable luminescence of the dimer achieves the purpose of increasing the number of luminescence bands and broadening the spectrum.
[0005] The technical solution adopted by the present invention to solve the above technical problems is:
[0006] The invention discloses a dual-phase nanocrystalline glass-ceramic material with multi-spectral broadband tunable luminescence. The composition formula of the glass matrix of the glass-ceramic material is (65-z)SiO2-zGa2O3-5Li2O-25ZnF2-5KF, wherein z is the molar fraction and the value of z is 2.5-17.5. Zn2SiO4 nanocrystals and ZnGa2O4 nanocrystals are precipitated in the glass matrix. Mn is doped in the glass matrix. 2+ With Cr 3+ , where Mn 2+ Doped in the form of MnCO3, Cr 3+ Doped in the form of Cr2O3, Mn 2+ The doping concentration is 0~3.0mol%Cr 3+ The doping concentration is 0~0.1mol%, and the doped Cr 3+ The doped Mn 2+ Selectively embedded into the [ZnO4] tetrahedral structure in Zn2SiO4 nanocrystals.
[0007] The invention provides a dual-phase nanocrystal glass-ceramic material with multi-spectral broadband tunable luminescence. The content of Ga2O3 in the glass matrix is adjustable within the range of 2.5-17.5 mol%. By adjusting the Ga2O3 content, the precipitation ratio of Zn2SiO4 and ZnGa2O4 dual-phase nanocrystals and the relative intensity of their luminescence bands can be adjusted. At the same time, when the Ga2O3 content is fixed, the Mn 2+The doping concentration can not only regulate the fluorescence intensity of the luminescent ions, but also cause changes in the number of luminescent bands.
[0008] Ga in ZnGa2O4 nanocrystals 3+ The radius (r = 62.0 pm) and the luminescent ion Cr 3+ The radius (r = 61.5 pm) is similar, and ZnGa2O4 nanocrystals can be Cr 3+ Providing a suitable octahedral coordination environment, so that the doped Cr 3+ It selectively embeds into the [GaO6] octahedral coordination structure in ZnGa2O4 nanocrystals, resulting in a red emission band at ~693nm. 2+ (radius r = 67.0 pm) and Zn 2+ (radius r = 74.0 pm) with the same valence and similar radius, and Zn2SiO4 nanocrystals contain [ZnO4] tetrahedron, which is Mn 2+ Provides a tetrahedral crystal field environment, so that the doped Mn 2+ Selectively embedded into the [ZnO4] tetrahedral structure in Zn2SiO4 nanocrystals, resulting in a green emission band.
[0009] Although [ZnO4] tetrahedrons also exist in ZnGa2O4 nanocrystals, in the dual-phase nanocrystalline glass-ceramic material of the present invention, Mn 2+ Only preferentially and selectively embed into the [ZnO4] tetrahedral structure of Zn2SiO4 nanocrystals, while Cr 3+ Selectively embedded into the [GaO6] octahedral coordination structure in ZnGa2O4 nanocrystals, that is, Mn 2+ and Cr 3+ They exist in Zn2SiO4 nanocrystals and ZnGa2O4 nanocrystals respectively, achieving local spatial isolation of Mn 2+ and Cr 3+ The effect of Mn 2+ and Cr 3+ Luminescence quenching due to energy transfer.
[0010] The Zn2SiO4 nanocrystals and ZnGa2O4 nanocrystals precipitated in the glass matrix of the glass-ceramic material of the present invention can be transition metal ions Mn 2+ and Cr 3+ Providing a suitable luminescent coordination environment, by changing the Ga2O3 content from 2.5mol% to 17.5mol%, the transformation of the nanocrystals from Zn2SiO4 single phase to Zn2SiO4 / ZnGa2O4 dual phase can be regulated, thereby obtaining the Mn 2+ and Cr3+ The spectral composition covers tunable multi-band composite broadband luminescence from 475 to 800 nm.
[0011] Furthermore, Mn 2+ The doping concentration is 0.2~3.0mol%Cr 3+ The doping concentration is 0.01 to 0.1 mol%.
[0012] Changing the ion doping concentration not only affects the luminescence intensity, but also causes the number of luminescence bands to change. 2+ The doping concentration of Mn is less than 1.5 mol%, and a green luminescence band and a red luminescence band are generated in the glass ceramic material; 2+ The doping concentration is ≥ 1.5 mol % and a green luminescence band, a red luminescence band and an orange luminescence band are generated in the glass ceramic material. For example, when the Ga2O3 content in the glass matrix of the glass ceramic material of the present invention is fixed to 10 mol %, two-phase nanocrystals of Zn2SiO4 and ZnGa2O4 are precipitated in the glass matrix. 2+ When the doping concentration is less than 1.5 mol%, under 422 nm blue light excitation, Mn 2+ Emitting ~530nm green light peak, Cr 3+ The red emission peak of 693 nm is emitted, so that the central wavelength of 530 nm (Mn 2+ ) and ~693nm(Cr 3+ ) at the continuous double emission band (i.e., green and red emission bands), and when Mn 2+ When the doping concentration of ≥1.5mol%, a new emission band ~609nm (i.e. orange emission band) will be superimposed in the above spectrum. The emission bands with different centers can cover the ultra-wideband emission of 475-800nm.
[0013] Specifically, Zn2SiO4 nanocrystals are formed with Mn 2+ -Mn 2+ Dimer.
[0014] Specifically, two [ZnO4] tetrahedrons connected in Zn2SiO4 nanocrystals are connected by O 2- The structure makes the two Zn in two adjacent [ZnO4] tetrahedrons 2+ The distance between Satisfy the formation of Mn 2+ -Mn 2+ Critical conditions for ion pairs Therefore, in Mn 2+ At high doping concentrations of ≥1.5mol%, more Mn 2+Can enter Zn2SiO4 nanocrystals, two Zn in two adjacent [ZnO4] tetrahedrons 2+ Mn 2+ -Mn 2+ Ion pair, namely Mn 2+ -Mn 2+ Dimer, the Mn 2+ -Mn 2+ The dimer acts as a new luminescent center, thereby generating an additional orange emission band at ∼609 nm.
[0015] Compared with the prior art, the present invention has the following advantages:
[0016] 1) The present invention has a multi-spectral broadband tunable luminescent dual-phase nanocrystalline glass ceramic material, wherein Zn2SiO4 nanocrystals and ZnGa2O4 nanocrystals are precipitated in the glass matrix and co-doped with transition metal ions Mn 2+ and Cr 3+ , achieving tunable multi-band composite broadband luminescence covering 475-800nm. And by high concentration doping of Mn 2+ The strategy can promote new luminescence centers (i.e., Mn 2+ -Mn 2+ dimer), realizing the single Mn 2+ To Mn 2+ -Mn 2+ The adjustable luminescence of the dimer achieves the purpose of increasing the number of luminescence bands and broadening the spectrum.
[0017] 2) The content of Ga2O3 in the glass matrix of the glass-ceramic material of the present invention is adjustable within the range of 2.5 to 17.5 mol%. By adjusting the Ga2O3 content, the precipitation ratio of Zn2SiO4 and ZnGa2O4 dual-phase nanocrystals and the relative intensity of their luminescence bands can be adjusted. At the same time, when the Ga2O3 content is fixed, by adjusting the Mn 2+ The doping concentration can not only regulate the fluorescence intensity of the luminescent ions, but also cause changes in the number of luminescent bands.
[0018] 3) Mn 2+ and Cr 3+ They exist in Zn2SiO4 nanocrystals and ZnGa2O4 nanocrystals respectively, achieving local spatial isolation of Mn 2+ and Cr 3+ The effect of Mn 2+ and Cr 3+ Luminescence quenching due to energy transfer.
[0019] 4) Changing the ion doping concentration not only affects the luminescence intensity, but also causes the number of luminescence bands to change. Specifically, Mn 2+ The doping concentration of Mn is less than 1.5 mol%, and a green luminescence band and a red luminescence band are generated in the glass ceramic material; 2+ The doping concentration is ≥1.5 mol % and a green emission band, a red emission band and an orange emission band are generated in the glass ceramic material. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The XRD patterns of the glass ceramic samples of Comparative Example 1 and Examples 1 to 4 and the standard diffraction cards of Zn2SiO4 and ZnGa2O4 nanocrystals;
[0021] Figure 2 The luminescence spectra of the glass ceramic samples of Comparative Example 1 and Examples 1 to 4;
[0022] Figure 3 The luminescence spectra of the glass ceramic samples of Comparative Example 2 and Examples 5 to 7;
[0023] Figure 4 The XRD patterns of the glass-ceramic samples of Comparative Example 3 and Example 8 and the standard diffraction card of Zn2SiO4 nanocrystals;
[0024] Figure 5 It is the luminescence spectrum diagram of the glass ceramic samples of Comparative Example 3 and Example 8. DETAILED DESCRIPTION
[0025] The present invention is further described in detail below with reference to Examples 1 to 8 and Comparative Examples 1 to 3 of the accompanying drawings.
[0026] 1. Embodiments 1 to 8
[0027] The dual-phase nanocrystalline glass-ceramic materials with multi-spectral broadband tunable luminescence of Examples 1 to 8 are all prepared by the following method:
[0028] 1) Raw material preparation: various raw materials are taken according to the proportion, mixed and ground evenly in an agate mortar to obtain 10g of the mixture, and carefully transferred to a high-purity quartz crucible; among them, SiO2 comes from Sinopharm Company with a purity of 99%, and other raw materials are from Aladdin Company with a purity of 99.99%;
[0029] 2) Melting and quenching: Place the high-purity quartz crucible containing the raw materials into a vertical heating furnace set at 1550°C in advance, then keep the high-purity quartz crucible at 1550°C for 30 minutes, then quickly pour the melt in the high-purity quartz crucible onto a stainless steel plate preheated to 200°C, and quickly press another stainless steel plate preheated to 200°C on the melt to complete the quenching process to obtain a solid block glass;
[0030] 3) Annealing: placing the solid block glass in an annealing furnace for annealing at a temperature of 400°C for 3 hours, and finally cooling naturally to room temperature to obtain a precursor glass;
[0031] 4) Heat treatment: Cut the precursor glass into 8 small glass samples of uniform shape and size, and then put them into an annealing furnace for heat treatment at 720°C for 5 hours, and finally cool them down to room temperature naturally;
[0032] 5) Polishing: The mold is ground on sandpaper with roughness of 1000 mesh, 2000 mesh and 4000 mesh, and finally polished with polishing paper and polishing solution to make both sides smooth and flat, and finally obtain a glass ceramic sample with uniform shape and size (thickness 2mm).
[0033] The reason for using high-purity quartz crucibles in the above preparation process is that high-purity quartz crucibles have the advantages of high purity, stable quality, and invariance at high temperatures. Compared with alumina crucibles (corundum crucibles), they can effectively prevent Al2O3 in alumina crucibles from corroding the glass melt during the experiment, which will have an adverse effect on subsequent experimental results. Therefore, high-purity quartz crucibles are used for melting in all the above preparation processes. In addition, the role of annealing is to remove internal stress to ensure good mechanical processing properties of the glass.
[0034] The vertical heating furnace adopts the SJF1700 vertical resistance furnace manufactured by Nanjing Boyuntong Company, and the annealing and heat treatment adopts the LT 5 / 11 / P330 precision annealing furnace manufactured by Nabertherm Company of Germany.
[0035] 2. Comparative Examples 1 to 3
[0036] Comparative Example 1: The difference from Examples 1 to 4 is that the Ga2O3 content in the glass matrix component is different. At this Ga2O3 content, only single-phase Zn2SiO4 nanocrystals are precipitated in the glass.
[0037] Comparative Example 2: The difference from Examples 5 to 7 is that the Mn in the glass matrix 2+ The doping concentration is different.
[0038] Comparative Example 3: The difference from Example 8 is that no heat treatment is performed and no nanocrystals are precipitated in the glass.
[0039] The differences in the naming, components and preparation conditions of the glass ceramic materials of Examples 1 to 4 and Comparative Example 1 are shown in Table 1. The differences in the naming, components and preparation conditions of the glass ceramic materials of Examples 5 to 7 and Comparative Example 2 are shown in Table 2. The differences in the naming, components and preparation conditions of the glass ceramic materials of Example 8 and Comparative Example 3 are shown in Table 3.
[0040] Table 1
[0041]
[0042] Table 2
[0043]
[0044] Table 3
[0045]
[0046] 3. Experimental Results Analysis
[0047] The above embodiments and comparative examples were subjected to performance tests. Figure 1 The XRD patterns of the glass ceramic samples of Comparative Example 1 and Examples 1 to 4 and the standard diffraction cards of Zn2SiO4 and ZnGa2O4 nanocrystals are shown in FIG. Figure 1 It can be seen in comparative example 1 that its crystallization peak is very consistent with the standard card of Zn2SiO4 nanocrystals (JCPDS No.8-492), proving that the precipitated crystals are Zn2SiO4 nanocrystals. As the Ga2O3 content increases from 2.5mol% to 17.5mol%, the diffraction intensity of the weak diffraction peak at 35.85° increases significantly, and after comparison with the standard card, it is determined to be the diffraction peak of ZnGa2O4 nanocrystals (JCPDS No.38-1240). And the diffraction peak continues to increase with the increase of Ga2O3 content, indicating that the crystallization degree of ZnGa2O4 nanocrystals in the glass-ceramic sample continues to increase. On the contrary, the diffraction peak corresponding to the Zn2SiO4 nanocrystals continues to weaken with the increase of Ga2O3 content, indicating that the crystallization degree of Zn2SiO4 nanocrystals in the glass-ceramic sample continues to weaken (Examples 1 to 4). The reason for the above phenomenon is that when the Ga2O3 content is low, the free Ga in the precursor glass 3+ The content is relatively small, and after heat treatment, it is mixed with Zn 2+ The number of ZnGa2O4 nuclei formed is limited, resulting in less ZnGa2O4 crystal precipitation and relatively weak crystal diffraction peak intensity. 3+ The content continues to increase. When subjected to high temperature heat treatment, Zn 2+ with Ga 3+The probability of rapid diffusion to form ZnGa2O4 nuclei increases, which in turn leads to an increase in the precipitation of ZnGa2O4 nanocrystals in the glass matrix. 2+ The number of Zn2SiO4 nuclei formed with [SiO4] decreases, resulting in a decrease in the crystallinity of the formed Zn2SiO4 crystals during the subsequent crystal growth process. The above phenomenon shows that increasing the content of Ga2O3 in the invention can regulate the evolution of nanocrystals from single-phase Zn2SiO4 to dual-phase ZnGa2O4 / Zn2SiO4, thereby successfully obtaining dual-phase glass ceramics.
[0048] Figure 2 The luminescence spectra of the glass ceramic samples of Comparative Example 1 and Examples 1 to 4 are shown in FIG. 1. In Comparative Example 1, a single green emission band appears at 530 nm, corresponding to Mn 2+ of 4 T1( 4 G) → 6 A1( 6 S) radiative transition. With the increase of Ga2O3 content (Comparative Examples 1-4), red light emission at ~693nm begins to appear in the glass-ceramic samples, which originates from Cr 3+ of 2 E g → 4 A2 radiation transition. In Examples 2 to 4, multi-peak emission appears in the green light band, and the central wavelengths are located at 506nm and 530nm respectively after Gaussian peak separation ( Figure 2 (b)), indicating that Mn 2+ The above phenomenon is caused by the following reasons: in Comparative Example 1, only Zn2SiO4 nanocrystals are precipitated, and Mn 2+ Entering the Zn2SiO4 lattice and located in the tetrahedral crystal field, it produces green light emission at ~530nm. 3+ The luminescent coordination environment, at this time Cr 3+ It is difficult for it to enter the Zn2SiO4 crystal to produce light. As the Ga2O3 content increases (Examples 1 to 4), ZnGa2O4 crystals begin to precipitate and the degree of crystallization continues to increase. More Cr 3+ Entering into ZnGa2O4 nanocrystals, the ~693nm red light emission is continuously enhanced. The precipitation of Zn2SiO4 crystals in the glass is continuously reduced, so Mn 2+ The luminescence at 530nm gradually weakens. In addition, when the Ga2O3 content is ≥15mol%, the crystallization degree of ZnGa2O4 crystal is significantly greater than that of Zn2SiO4. Due to the reduction of Zn2SiO4 crystals, Mn 2+It begins to enter the ZnGa2O4 lattice in a tetrahedral crystal field, thereby producing green light emission at ~506nm. The above phenomenon proves that Zn2SiO4 and ZnGa2O4 are Mn 2+ Provides a tetrahedral luminescent environment, while only ZnGa2O4 nanocrystals are Cr 3+ Provides an octahedral luminous environment.
[0049] Figure 3 The luminescence spectra of the glass ceramic samples of Comparative Example 2 and Examples 5 to 7 are shown in Figure 2. Under 422 nm wavelength excitation, Mn 2+ The intensity of the characteristic emission spectrum of Mn increases first and then decreases with the increase of doping concentration. 2+ When the concentration is 1.5mol%, the strongest emission is achieved. This phenomenon can be attributed to the 2+ With the increase of Mn concentration 2+ -Mn 2+ The distance between them is reduced, thus causing the concentration quenching effect. And in Comparative Example 2, Mn 2+ The characteristic emission is only in the green band at ~530nm, which is due to the fact that Zn2SiO4 is Mn 2+ Provide a tetrahedral luminescence environment, that is, in this sample, Mn 2+ Preferentially selectively embedded in Zn2SiO4 nanocrystals. In Examples 5 to 7 (increasing Mn 2+ There are two possible sources of this orange emission peak, namely, the Mn 2+ Emission or Mn 2+ -Mn 2+ The luminescence produced by the dimer. In ZnGa2O4 crystal, Ga 3+ Occupies a six-coordinated octahedral crystal field environment, but in the case of ZnGa2O4:Mn 2+ Mn has not been observed in the reports of the system 2+ The orange luminescence of Mn 2+ Enter into ZnGa2O4 nanocrystals and occupy Ga 3+ On the other hand, in the ZnGa2O4 unit cell, two adjacent Zn 2+ They do not share anions and are not sufficient to produce Mn 2+ -Mn 2+ The orange emission peak is attributed to the Mn in Zn2SiO4 nanocrystals. 2+ -Mn 2+ The above phenomenon once again illustrates that the dual-phase glass ceramics of the present invention change Mn 2+ The doping concentration can not only regulate the change of spectral intensity, but also cause changes in the number of emission bands.
[0050] In order to further illustrate the origin of the orange luminescence peak at 609 nm, the XRD patterns of the glass ceramic containing only Zn2SiO4 nanocrystalline (Example 8) and the precursor sample (Comparative Example 3) were compared. Figure 4 ) and spectrogram ( Figure 5 ).from Figure 4 It can be seen that the crystallization peak in Example 8 is very consistent with the standard diffraction card of Zn2SiO4 nanocrystals, indicating that the crystals precipitated in the sample are Zn2SiO4, and the high concentration of Mn 2+ Doping does not induce phase change. Figure 5 In the comparative example 3 sample, only the red light emission peak at the peak value of 660 nm is present, which corresponds to the Mn 2+ Luminescence. After heat treatment, dual broadband emission appeared in Example 8, and the peaks were located at 530nm and 609nm respectively after Gaussian fitting. In the unit cell structure of ZnSiO4 nanocrystals, the two connected [ZnO4] tetrahedrons have a common point (O 2- ) are connected, and this structure makes two adjacent Zn 2+ The distance between Satisfy the formation of Mn 2+ -Mn 2+ Critical conditions for ion pairs When Mn 2+ Enters into Zn2SiO4 nanocrystals, partially replacing Zn in [ZnO4] 2+ lattice site, directly emitting green light at ~530nm. 2+ As the doping concentration increases, the Mn that enters the Zn2SiO4 nanocrystals 2+ More and more, greatly shortening Mn 2+ The distance between them promotes the formation of Mn 2+ (Zn 2+ )-Mn 2+ (Zn 2+ ) dimer becomes a new luminescent center, and finally passes through [ 6 A1( 6 S) 4 T1( 4 G)]→[ 6 A1( 6 S) 6 A1( 6 The S)] hybrid state transition emits orange light at ~609nm.
Claims
1. A dual-phase nanocrystalline glass-ceramic material having multi-spectral broadband tunable luminescence, characterized in that: The glass matrix of the glass ceramic material has a composition formula of (65-z)SiO2-zGa2O3-5Li2O-25ZnF2-5KF, wherein z is a molar fraction, and the value of z is 2.5-17.
5. Zn2SiO4 nanocrystals and ZnGa2O4 nanocrystals are precipitated in the glass matrix, and Mn is doped in the glass matrix. 2+ With Cr 3+ , where Mn 2+ Doped in the form of MnCO3, Cr 3+ Doped in the form of Cr2O3, Mn 2+ The doping concentration is 0~3.0mol%Cr 3+ The doping concentration is 0~0.1mol%, and the doped Cr 3+ The doped Mn 2+ Selectively embedded into the [ZnO4] tetrahedral structure in Zn2SiO4 nanocrystals.
2. The dual-phase nanocrystalline glass-ceramic material with multi-spectral broadband tunable luminescence according to claim 1, characterized in that: Mn 2+ The doping concentration is 0.2~3.0mol%Cr 3+ The doping concentration is 0.01 to 0.1 mol%.
3. The dual-phase nanocrystalline glass-ceramic material with multi-spectral broadband tunable luminescence according to claim 1 or 2, characterized in that: Mn 2+ The doping concentration is less than 1.5 mol % and a green emission band and a red emission band are generated in the glass ceramic material.
4. The dual-phase nanocrystalline glass-ceramic material with multi-spectral broadband tunable luminescence according to claim 1 or 2, characterized in that: Mn 2+ The doping concentration is ≥1.5 mol % and a green emission band, a red emission band and an orange emission band are generated in the glass ceramic material.
5. The dual-phase nanocrystalline glass-ceramic material with multi-spectral broadband tunable luminescence according to claim 4, characterized in that: Mn is formed in Zn2SiO4 nanocrystals 2+ -Mn 2+ Dimer.
6. The dual-phase nanocrystal glass-ceramic material with multi-spectral broadband tunable luminescence according to claim 5, wherein two [ZnO4] tetrahedrons connected in the Zn2SiO4 nanocrystal are connected by O 2- The two Zn in two adjacent [ZnO4] tetrahedrons are connected at the same point. 2+ The distance between The two Zn in two adjacent [ZnO4] tetrahedrons 2+ Mn 2 + -Mn 2+ The ion pair is the Mn 2+ -Mn 2+ Dimer.
Citation Information
Patent Citations
Ultra-wideband near-infrared luminous transparent glass-ceramic
CN101353228A