A high content YB 4 Preparation method of doped C / C composite material
Through the cyclic heat treatment process, YB4 is introduced into C/C composite materials at a high content, which solves the stability of the material in a high-temperature oxidation environment, and improves the oxidation and ablation resistance, simplifies the process and reduces costs.
Patent Information
- Application Number
- CN202310821653.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-07-06
AI Technical Summary
The existing C/C composite materials are prone to oxidation and fall off under high-temperature oxidation environments, which limits their application in the aerospace field, especially due to the huge thermal expansion difference between rare earth-based borides and carbon materials, which leads to the temperature change of coating structure. Unstable.
By preparing boron source liquid phase and yttrium-carbon source liquid phase pioneers, YB4 is introduced into the C/C composite material, and a cyclic heat treatment process is adopted, including low-temperature, medium-temperature and high-temperature heat treatment, to improve the content and uniformity of YB4 and enhance the anti-oxidation resistance and ablation resistance.
The uniform consolidation of high content YB4 is achieved, which significantly improves the oxidation resistance and ablation resistance of C/C composite materials, reduces the preparation cost, and simplifies the process flow, ensuring the stability of the material in a high-temperature environment.
Smart Images

Figure CN116891385B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of C / C composite materials, and in particular to a high-content YB 4 The invention discloses a method for preparing a doped C / C composite material. Background Art
[0002] C / C composites are ideal high-temperature materials with low density, high specific strength, ablation resistance, excellent mechanical properties and high-temperature stability. Therefore, this material has extremely high application value in the aerospace field. Limited by the easy oxidation characteristics of carbon materials, that is, oxidation occurs at temperatures above 400°C and violent oxidation occurs above 600°C, its service ability in aerobic environments is extremely poor, which seriously restricts the engineering application of C / C composites. The effective introduction of ultra-high temperature ceramics (UHTCs) to prepare C / C-UHTCs composites, such as C / C-SiC-ZrC and C / C-HfC, can effectively improve the high-temperature performance of C / C composites. The oxides (Y 2 O 3 ) can inhibit the phase change process of Zr and Hf-based oxides, thereby further enhancing the antioxidant and ablation resistance of C / C-UHTCs composites. Therefore, its combination with C / C composites has received widespread attention.
[0003] Limited by yttrium boride (YB 4 / YB 6 ) has an extremely high melting point (higher than 2300℃) and is difficult to dissolve in any inorganic or organic solvents. Its application is mostly concentrated in the preparation of C / C composite coating structures by embedding method, plasma sintering method, spraying method, etc., and the corresponding preparation process has become increasingly mature. However, due to the huge thermal expansion difference between rare earth borides and carbon materials, the prepared coating structure is easily oxidized and then eroded or falls off when the temperature changes at a large gradient. Therefore, the stability of the component in a strong ablation or cyclic ablation environment is limited. Using matrix modification technology to convert (YB 4 / YB 6 The more mature processes for introducing ) into C / C composite materials include spraying process, which is to introduce (YB 4 / YB 6 ) The powder is sprayed layer by layer and then woven to construct a repeating structure of non-woven fabric layer-mesh layer-powder layer. The cost of this method is relatively low, but the amount of powder introduced is low and the distribution uniformity is poor, which greatly limits the (YB 4 / YB 6 )Application of matrix modification. Summary of the invention
[0004] (I) In view of the shortcomings of the prior art, the present invention provides a high-content YB 4The preparation method of the doped C / C composite material overcomes the shortcomings of the prior art and effectively solves the problems mentioned in the above background.
[0005] (II) To achieve the above objectives, the present invention is implemented by the following technical solutions: a high content YB 4 The preparation method of the doped C / C composite material comprises the following steps:
[0006] (1) preparing a boron source liquid precursor and a yttrium-carbon source liquid precursor;
[0007] (2) The C / C preform is immersed in a boron source and a yttrium-carbon source liquid precursor successively and subjected to low temperature heat treatment, and then subjected to medium temperature heat treatment after three cycles, and then subjected to high temperature heat treatment after three cycles, to obtain C / C-YB 4 Composite materials.
[0008] Preferably, in step (1), the boron source liquid precursor is H 3 BO 3 (boric acid)-propylene glycol-alcohol in a volume ratio of 1: (3-5): (3-8); the yttrium-carbon source liquid precursor is YCl 3 6H 2 O(Yttrium chloride hexahydrate)-C 6 H 12 O 6 (Glucose) was dissolved in deionized water at a mass ratio of 2:1.
[0009] Preferably, in step (2), the low-temperature heat treatment temperature is 800-1000°C, the medium-temperature heat treatment temperature is 1400-1600°C, and the high-temperature heat treatment temperature is 1700-1900°C.
[0010] Preferably, the C / C-YB 4 The specific process of composite materials is as follows:
[0011] A1: Hanging the carbon fiber blank in a chemical vapor deposition furnace, introducing pyrolytic carbon into the carbon fiber blank by chemical vapor deposition process, and obtaining a C / C preform with a porous structure; A2: Impregnating the C / C preform in a boron source liquid precursor, placing it in a drying box for drying, and heat-insulating it in a high-temperature furnace, the process is repeated 3 times, and a boron-containing C / C preform is obtained; A3: Impregnating the boron-containing C / C preform in a yttrium-carbon source liquid precursor, placing it in a drying box for drying, and heat-insulating it in a high-temperature furnace, the process is repeated 3 times, and a yttrium-carbon-boron modified C / C preform blank is obtained; A4: After the yttrium-carbon-boron modified C / C preform is subjected to medium-temperature heat treatment, it is first immersed in a boron source liquid precursor, dried, and then immersed in a yttrium source liquid precursor, dried, and then subjected to medium-temperature heat treatment, and the process is repeated 3 times and then subjected to high-temperature heat treatment, and C / C-YB4 Composite materials.
[0012] Preferably, in step A1, the chemical vapor deposition process is: the carbon source gas and the carrier gas are propylene and nitrogen respectively, the flow ratio of propylene to nitrogen is 4:3, the deposition pressure is ≤10 kPa, and the deposition temperature is 800-1000°C.
[0013] Preferably, in step A2, the boron source liquid precursor contains H 3 BO 3 -The volume ratio of propylene glycol to alcohol is 1:3:4; the drying temperature is controlled at 80 and 110°C for 2 hours each, then increased to 150°C for 3-8 hours; the insulation temperature is 600-700°C.
[0014] Preferably, in step A3, the drying temperature is controlled to be 80 and 110°C for 2 hours each, and then increased to 100-200°C for 3-8 hours; the insulation temperature is 800-1000°C.
[0015] Preferably, in step A4, the heat treatment process is as follows: heating to 350°C and 700°C and keeping them for 30-60 min each, then raising the temperature to 1200-1900°C and keeping them for 1-3 h, during which the heating rate is controlled at 2-3°C / min.
[0016] The present invention also provides C / C-YB 4 Another method for preparing the composite material is as follows:
[0017] B1: Hanging the carbon fiber blank in a chemical vapor deposition furnace, introducing pyrolytic carbon into the carbon fiber blank by chemical vapor deposition process, and obtaining a C / C preform with a porous structure; B2: Impregnating the C / C preform in a boron source liquid precursor, placing it in a drying box for drying, and heat-insulating it in a high-temperature furnace, the process is repeated twice, and a boron-containing C / C preform is obtained; B3: Impregnating the boron-containing C / C preform in a yttrium-carbon source liquid precursor, placing it in a drying box for drying, and heat-insulating it in a high-temperature furnace, the process is repeated twice, and a yttrium-carbon-boron modified C / C preform blank is obtained; B4: After the yttrium-carbon-boron modified C / C preform is subjected to medium-temperature heat treatment, it is first impregnated in a boron source liquid precursor, dried, and then impregnated in a yttrium-carbon source liquid precursor, dried, and then subjected to medium-temperature heat treatment, and the process is repeated twice and then subjected to high-temperature heat treatment, and C / C-YB 4 Composite materials.
[0018] Preferably, in step B2, the boron source liquid precursor is H 3 BO 3 -C 3 H 7NO (dimethylformamide) in a mass ratio of 1: (2-5); control the drying temperature to be 100-200°C for 3-8h; keep the temperature at 500-800°C; in step B3, the yttrium-carbon source liquid precursor is YCl 3 -PF(phenolic resin)-C 3 H 7 NO is composed in a mass ratio of 4:1:(5-8); the drying temperature is controlled to be 150-350°C for 3-8h; the insulation temperature is 800-1200°C.
[0019] (III) The present invention provides a high content YB 4 The preparation method of the doped C / C composite material has the following beneficial effects:
[0020] 1. The present invention uses YCl 3 6H 2 O, H 3 BO 3 , C 6 H 12 O 6 As a precursor, YB was reduced by carbothermal and boronthermal methods. 4 Introduce carbon fiber into the blank to achieve YB inside the C / C composite matrix 4 A breakthrough in content, YB 4 The content can reach 33.52%, and it is uniformly consolidated in the matrix, thereby improving the oxidation resistance and ablation resistance of the C / C-based composite material. This method also has the characteristics of low cost, simple operation, safety and reliability.
[0021] 2. In the drying process of the present invention, the temperature is increased to 150℃ for 5h, and the temperature is 80℃ and 110℃ for 2h respectively. 3 BO 3 During decomposition, the loss of boron source and carbon source in the green body can be reduced.
[0022] 3. In the heat treatment process of the C / C preform of the present invention, after three heat treatments at 1400°C, the temperature is then raised to 1800°C and kept warm, in order to prevent excessive intermediate products of the precursor, and excessive expansion of the volume of the ceramic product during the cracking of the precursor, thereby destroying the structure of the preform.
[0023] 4. C / C-YB provided by the present invention 4 Composite material, using C 3 H 7 NO instead of C 3 H 8 O 3 and H 2 O as solvent to disperse H 3 BO 3and YCl 3 , solved H 3 BO 3 -C 3 H 7 The viscosity of NO solution is difficult to adjust, and the impregnation efficiency of boron source and yttrium-carbon source is further improved, shortening the preparation cycle of the composite material. However, the yttrium source used is anhydrous YCl 3 , the cost of this precursor is significantly higher than that of YCl 3 6H 2 O. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 C / C-YB in Example 1 of the present invention 4 XRD spectra of the composite materials;
[0025] Figure 2 C / C-YB in Example 1 of the present invention 4 Microscopic morphology and surface scanning analysis results of preform composite materials: (a) C / C-YB 4 Microscopic cross-sectional morphology after treatment at 1800℃; (b) is the morphology of the ceramic phase distribution between fiber bundles; (c) is the ceramic morphology in the matrix; (df) are the distribution diagrams of Y, C, and O elements in the ceramic phase, respectively.
[0026] Figure 3 C / C-YB provided in Example 3 of the present invention 4 -XRD spectrum of HfC composite material: X is YB introduced by weaving process 4 Modified C / C-HfC composite material comparison sample; Y C / C-YB prepared by the process of the present invention 4 -HfC composite materials.
[0027] Figure 4 C / C-YB in Example 3 of the present invention 4 -HfC composite microstructure and surface scanning analysis results: (a) C / C-YB 4 -HfC composite material micromorphology; (b) is the micromorphology of the local magnified image; (c) is the magnified ceramic structure morphology; (df) are the Hf, Y, and C element distribution diagrams of the ceramic phase, respectively. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0029] Example 1
[0030] A C / C-YB 4 The preparation method of the composite material is as follows:
[0031] A1: 0.45g / cm 3 The needle-punched carbon fiber blank was suspended in a chemical vapor deposition furnace, and pyrolytic carbon was introduced into the carbon fiber blank by chemical vapor deposition process to obtain a density of 0.58g / cm 3 The porous structure C / C preform is prepared by chemical vapor deposition process, wherein the carbon source gas and the carrier gas are propylene and nitrogen respectively, the flow ratio of propylene and nitrogen is 4:3, the deposition pressure is 2 kPa, and the deposition temperature is 1000°C.
[0032] A2: The C / C preform is immersed in a boron source liquid precursor, placed in a drying oven for drying, and then heat-insulated in a high-temperature furnace. The process is repeated 3 times to obtain a boron-containing C / C preform. 3 BO 3 -The volume ratio of propylene glycol to alcohol is 1:3:4; the drying temperature is controlled at 80 and 110°C for 2 hours each, then increased to 150°C for 5 hours; the insulation temperature is 700°C.
[0033] A3: The boron-containing C / C preform is immersed in a yttrium-carbon source liquid precursor, placed in a drying oven for drying, and then kept in a high-temperature furnace for heat preservation. The process is repeated 3 times to obtain a yttrium-carbon-boron modified C / C preform. 3 6H 2 OC 6 H 12 O 6 -H 2 O, and YCl 3 6H 2 OC 6 H 12 O 6 -H 2 The mass ratio of O is 1:2:6; the drying temperature is controlled at 80 and 110°C for 2 hours each, and then increased to 150°C for 5 hours; the insulation temperature is 800°C.
[0034] A4: After medium-temperature heat treatment of the yttrium-carbon-boron modified C / C preform body, it is first immersed in a boron source liquid precursor, and then dried for low-temperature heat treatment, and then immersed in a yttrium source liquid precursor, and then dried for heat treatment. The boron and yttrium source processes are introduced and cycled for 3 times each. The heat treatment process is as follows: heating to 350°C and keeping warm for 40 minutes, then performing low-temperature heat treatment at 700°C (boron source), and performing heat treatment at 1000°C (yttrium source), and the insulation time is 1 hour.
[0035] A5: After the heat treatment, the Y-C-B modified C / C preform is subjected to medium temperature heat treatment and then the A4 process is repeated. After three medium temperature heat treatments, high temperature heat treatment is performed to obtain a density of 1.25 g / cm 3 C / C-YB 4 The heat treatment process is as follows: heating to 1400°C for medium-temperature heat treatment and keeping the temperature for 1 hour, heating to 1800°C for high-temperature heat treatment and keeping the temperature for 2 hours, during which the heating rate is controlled at 2°C / min.
[0036] Figure 1 C / C-YB prepared in Example 1 4 Phase analysis of composite materials. Figure 1 C / C-YB 4 The XRD spectrum of the composite material shows that the peaks are narrow and sharp, indicating that the crystal structure of the ceramic phase in the matrix is complete, that is, the carbon thermal and boron thermal reactions are completely carried out. 4 As the main peak, accompanied by a small amount of YB 6 , YB 2 C 2 and YC 2 Phase, and YB 4 It is much higher than other phases, indicating that the yttrium-based precursor has basically completed the transformation to YB 4 The transformation of YB 2 C 2 and YC 2 The contents of the two in the matrix can be reduced or eliminated by further increasing the amount of boron source introduced.
[0037] Figure 2 C / C-YB prepared in Example 1 4 Cross-sectional morphology of the composite material and the corresponding surface scanning analysis of the ceramic. Figure 2 a shows that the generated ceramic phase is mainly distributed in the web layer of the C / C green body. 4 There are still a lot of unfilled pores inside the composite material. Zoom in on the fiber bundle area (area A), as shown in Figure 2 b shows that some nano-ceramic particles still exist between the fiber bundles. The ceramic in area B is magnified. Figure 2 c shows that the ceramic phases agglomerated and merged into a whole block of ceramics with a near-sintered structure. The energy spectrum analysis shows that ( Figure 2 d, e), the ceramic block is composed of a large amount of YB 4 and a small amount of YC 2 The ceramic block structure effectively eliminates the pores between ceramic particles and can provide a large number of impregnation channels for the subsequent densification of other ceramics, thereby improving the density of the subsequent composite material. Figure 2 The extremely low oxygen content in f verifies that the carbon thermal and boron thermal reactions in the matrix are completely carried out.
[0038] Example 2
[0039] Another C / C-YB 4 The preparation method of the composite material is as follows:
[0040] B1: 0.45g / cm 3 The needle-punched carbon fiber blank was suspended in a chemical vapor deposition furnace, and pyrolytic carbon was introduced into the carbon fiber blank by chemical vapor deposition process to obtain a density of 0.61g / cm 3 The porous structure C / C preform is obtained by chemical vapor deposition process, wherein the carbon source gas and the carrier gas are propylene and nitrogen respectively, the flow ratio of propylene and nitrogen is 4:3, the deposition pressure is 3kPa, and the deposition temperature is 850℃.
[0041] B2: The C / C preform is immersed in a boron source liquid precursor, placed in a drying oven for drying, and then kept warm in a high-temperature furnace. The process is repeated twice to obtain a boron-containing C / C preform. The boron source liquid precursor is H 3 BO 3 -C 3 H 7 NO, and H 3 BO 3 and C 3 H 7 The mass ratio of NO is 1:3; the drying temperature is controlled to be 150℃ for 5h; the insulation temperature is 600℃.
[0042] B3: The boron-containing C / C preform is immersed in a yttrium-carbon source liquid precursor, placed in a drying oven for drying, and then kept in a high-temperature furnace for heat preservation. The process is repeated twice to obtain a yttrium-carbon-boron modified C / C preform body. The yttrium-carbon source liquid precursor is YCl 3 -PF-C 3 H 7 NO, and YCl 3 -PF-C 3 H 7 The mass ratio of NO is 4:1:8; the drying temperature is controlled at 200°C for 5 hours; the insulation temperature is 1000°C.
[0043] B4: After heat treatment, the yttrium-carbon-boron modified C / C preform is immersed in a boron source liquid precursor, dried, and then immersed in a yttrium-carbon source liquid precursor. After drying, medium-temperature heat treatment is performed. The B2 and B3 processes are circulated and medium-temperature heat treatment is performed, and then high-temperature heat treatment is performed to obtain a density of 1.32 g / cm 3 C / C-YB 4Composite materials. The heat treatment process is as follows: heating to 350℃ and 700℃ for 60min each, then heating to 1400℃ for medium temperature heat treatment for 1h, cycling B2 and B3 processes and performing 1400℃ heat treatment twice, then heating to 1800℃ and keeping for 2h, during which the heating rate is controlled at 2℃ / min.
[0044] In Example 1, in step A2, the C / C preform needs to be impregnated and cracked three times. This treatment can increase the boron source content in the matrix and facilitate the subsequent boron thermal reaction of the composite material. 3 H 8 O 3 (propylene glycol) and C 2 H 5 The ratio of OH (alcohol) is used to adjust the viscosity of the solvent. If the viscosity is too high, the boron source is difficult to enter. If the viscosity is too low, the boron source content entering is too small, which affects the subsequent boron thermal reaction.
[0045] In this embodiment, H 3 BO 3 Directly dispersed in dimethylformamide, increasing the amount of boron source introduced during a single impregnation process, thereby reducing the impregnation cycle and increasing YB 4 The amount of YCl 3 -PF-C 3 H 7 The NO precursor increases the carbon source introduction, and the Cl-O gas generated during cracking is greatly reduced. However, the yttrium source used is anhydrous YCl 3 , its price is significantly higher than YCl 3 6H 2 OC 6 H 12 O 6 -H 2 O precursor.
[0046] Example 3
[0047] A C / C-YB 4 -The preparation method of HfC composite material is as follows:
[0048] (1) HfCl 4 6H 2 OC 6 H 12 O 6 Dissolve in deionized water to obtain HfC liquid precursor; among them, HfCl 4 6H 2 O and C 6 H 12 O 6 The mass ratio of HfCl is 5:1; 4 6H2 OC 6 H 12 O 6 and deionized water at a ratio of 1:2.
[0049] (2) C / C-YB 4 The composite material was immersed in HfC liquid precursor and heat treated at 1400℃, and then heat treated at 1800℃ for 3 cycles, and then heat treated for 1h to obtain C / C-YB 4 -HfC composite materials.
[0050] In this embodiment, the C / C-YB in Example 1 is used. 4 Composite materials.
[0051] Figure 3 C / C-YB prepared in Example 4 4 -HfC composite material (sample Y) and compared with the XRD spectrum of YB 4 Ceramic, and then the XRD spectrum of C / C composite material modified by the same introduction process HfC. As can be seen from the figure, C / C-YB prepared by HfC modification process 4 In the case of composite materials (sample X), the matrix composition of the composite material is HfC, HfB 2 and C, where HfB 2 The formation of YB in the matrix 4 and HfC, HfO 2 BC and BO exchange occurred. At the same time, it can be seen that there is no diffraction peak of yttrium-based ceramics in the spectrum of sample X, indicating that compared with hafnium-based ceramics and carbon components, YB 4 The relative content of C / C-YB prepared by the method of the present invention is relatively low; 4 In the XRD spectrum of the HfC composite material, in addition to the above three phases, YB 4 and Y 2 C 3 The diffraction peaks of 2 C 3 The appearance of BC and BO in the matrix proves the exchange process, and also shows that the composite material prepared by the present invention can effectively improve the YB 4 The content.
[0052] Figure 4 C / C-YB prepared in Example 4 4 -HfC composite cross-sectional morphology scan and ceramic corresponding surface scan analysis diagram. Figure 4 a It can be seen that the hafnium-based ceramic effectively fills the C / C-YB in Example 1. 4 The preform has pores, and the prepared composite material has high density. Figure 4b is an enlarged view of the ceramic phase. According to the contrast difference, the matrix ceramic can be divided into two main ceramic phases. The surface scanning analysis is as follows: Figure 4 As shown in df, the white and gray phases are hafnium-based ceramics (HfC, HfB 2 ) and yttrium-based ceramics (YB 4 , Y 2 C 3 ). Due to the BC and BO exchange in the composite matrix during the ceramic introduction stage, the hafnium-based ceramics gradually turn to YB 4 Ceramic blocks penetrate and adhesion occurs, such as Figure 4 c is shown in the enlarged view. This structure can effectively improve the density of the composite material.
[0053] The embodiments of the present invention disclose preferred embodiments, but are not limited thereto. A person skilled in the art can easily understand the spirit of the present invention based on the above embodiments and make different extensions and changes. However, as long as they do not deviate from the spirit of the present invention, they are all within the protection scope of the present invention.
Claims
1. A method for preparing a YB4-doped C / C composite material, characterized in that: The preparation method The following steps are included: (1) Hanging the carbon fiber blank in a chemical vapor deposition furnace, introducing pyrolytic carbon into the carbon fiber blank by chemical vapor deposition process to obtain a C / C preform with a porous structure; (2) immersing the C / C preform in a boron source liquid precursor, drying it in a drying oven, and then heat-treating it in a high-temperature furnace. The process is repeated three times to obtain a boron-containing C / C preform. (3) impregnating the boron-containing C / C preform into a yttrium-carbon source liquid precursor, drying it in a drying oven, and then heat-treating it in a high-temperature furnace. The process is repeated three times to obtain a yttrium-carbon-boron modified C / C preform green body; (4) After the yttrium-carbon-boron modified C / C preform is subjected to a medium-temperature heat treatment, it is first immersed in a boron source liquid precursor, and then immersed in a yttrium source liquid precursor after drying. After drying, it is subjected to a medium-temperature heat treatment. After the process is cycled three times, it is subjected to a high-temperature heat treatment to obtain a C / C-YB4 composite material; The boron source liquid phase precursor is composed of H3BO3-propylene glycol-alcohol in a volume ratio of 1: (3-5): (3-8), and the yttrium-carbon source liquid phase precursor is YCl3·6H2O-C6H 12 O6 is dissolved in deionized water in a mass ratio of 2:1; or the boron source liquid precursor is composed of H3BO3-C3H7NO in a mass ratio of 1:(2-5), and the yttrium-carbon source liquid precursor is composed of YCl3-PF-C3H7NO in a mass ratio of 4:1:(5-8).
2. The method for preparing a YB4-doped C / C composite material according to claim 1, wherein: In step (1), the chemical vapor deposition process is as follows: the carbon source gas and the carrier gas are propylene and nitrogen respectively, the flow ratio of propylene to nitrogen is 4:3, the deposition pressure is ≤10kPa, and the deposition temperature is 800-1000°C.
3. The method for preparing a YB4-doped C / C composite material according to claim 1, wherein: In step (2), when the volume ratio of H3BO3-propylene glycol-alcohol in the boron source liquid precursor is 1:3:4, the drying temperature is controlled to be 80 and 110°C for 2 hours each, and then increased to 150°C for 3-8 hours; the insulation temperature is 600-700°C.
4. The method for preparing a YB4-doped C / C composite material according to claim 3, wherein: In step (3), YCl3·6H2O-C6H 12 When O6 is dissolved in deionized water at a mass ratio of 2:1, the drying temperature is controlled to be 80 and 110°C for 2 hours each, and then increased to 100-200°C for 3-8 hours; the insulation temperature is 800-1000°C.
5. The method for preparing a YB4-doped C / C composite material according to claim 1, wherein: In step (2), when the boron source liquid precursor is composed of H3BO3-C3H7NO in a mass ratio of 1:(2-5), the drying temperature is controlled to be 100-200°C for 3-8h; and the insulation temperature is 500-800°C.
6. The method for preparing a YB4-doped C / C composite material according to claim 5, characterized in that: In step (3), when the yttrium-carbon source liquid precursor is composed of YCl3-PF-C3H7NO in a mass ratio of 4:1:(5-8); the drying temperature is controlled to be 150-350°C for 3-8h; and the insulation temperature is 800-1200°C.
7. The method for preparing a YB4-doped C / C composite material according to claim 1, wherein: In step (4), the heat treatment process is as follows: heating to 350°C and 700°C and keeping them for 30-60 minutes respectively, then raising the temperature to 1200-1900°C and keeping them for 1-3 hours, during which the heating rate is controlled at 2-3°C / min.