A Ti2AlC-Fe based wear-resistant self-lubricating coating and preparation method thereof

Through plasma spraying technology in the bore of the internal combustion engine cylinder, the Al element is used to form a solid solution phase in the MAX phase and regulate the spraying process, and a Ti2AlC-Fe-based wear-resistant self-lubricating coating is developed, which solves the problem of the combination of coatings in the bore of the cylinder. In order to solve the problems of insufficient strength and wettability, a coating with high microhardness and low friction coefficient is realized, which improves the wear resistance and self-lubricating performance of the inner wall of the cylinder.

CN116904910BActive Publication Date: 2024-10-01BEIJING JIAOTONG UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310632331.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-10-01
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

The existing plasma spray reinforced layer in the bore of the internal combustion engine cylinder has deficiencies in wettability and bonding strength, resulting in poor interface bonding and easy falling off. There are also internal defects such as holes and cracks, which affect the wear resistance and self-lubrication of the coating. performance.

Method used

In the MAX phase in which the A-site element is Al, the Al element is desolvated along the MAX phase crystal plane and diffuses to the metal matrix interface to form a new solid solution phase, and by regulating the inner hole rotation plasma spraying process and the raw material powder ratio , developed a Ti2AlC-Fe-based wear-resistant self-lubricating coating , including 80% to 95% Fe and 5% to 20% Ti2AlC, as well as FexOy, Ti3AlC2 and TiC formed after high temperature decomposition. Optimize spraying parameters such as spray gun rotation speed, vertical movement speed and air flow to improve the bonding of the coating. Strength and coefficient of friction.

Benefits of technology

A Ti2AlC-Fe-based wear-resistant self-lubricating coating with high microhardness, good tensile bonding strength and low friction coefficient has been achieved, which enhances the wear resistance and self-lubricating performance of the inner wall of the cylinder, reduces internal defects, and improves the coating's durability Quality and reusability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116904910B_ABST
    Figure CN116904910B_ABST
Patent Text Reader

Abstract

This invention relates to a Ti2AlC-Fe-based wear-resistant self-lubricating coating and its preparation method. The wear-resistant self-lubricating coating comprises the following raw materials by mass percentage: 80%–95% Fe, 5%–20% Ti2AlC; wherein the sum of the Fe and Ti2AlC components is 100%. This wear-resistant self-lubricating coating directly uses commercially available raw material powders as raw materials, making the raw material acquisition simple and low-cost, and possessing self-healing and reusable characteristics. The preparation method of this wear-resistant self-lubricating coating optimizes the internal rotating plasma spraying process and the raw material powder ratio; the method is simple, easy to operate, and suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of materials, and in particular to a Ti 2 AlC-Fe based wear-resistant self-lubricating coating and preparation method thereof. Background Art

[0002] In recent years, the energy conservation and emission reduction issues of internal combustion engines and the failure of frictional moving parts have continued to receive attention and concern. The wear failure of the cylinder block and piston ring of the internal combustion engine accounts for about 40% of the tribological failures of the entire machine, and the energy loss accounts for 60% of the total mechanical energy loss. Therefore, the development of new composite coatings to replace the heavy cylinder liners of internal combustion engines, achieve lightweight internal combustion engines to save energy, and improve tribological properties to extend the service life of internal combustion engines has significant economic benefits and practical significance.

[0003] The inner hole plasma spraying technology has significant advantages such as high economy, high forming efficiency, and good forming uniformity. It is the best technical means to prepare the inner hole strengthening layer of the internal combustion engine cylinder body to replace the traditional cast iron cylinder liner. However, the existing internal combustion engine cylinder body plasma spray strengthening layer has poor wettability with the cylinder body, poor interface bonding and easy to fall off. It is necessary to further design and optimize the coating components, enhance the bonding strength between the coating and the inner wall of the cylinder body and improve the wear resistance and self-lubricating performance of the coating; at the same time, optimize the plasma spraying preparation process of the coating, reduce internal defects such as holes and cracks, and improve the coating quality.

[0004] The graphite-like layered structure of the MAX phase gives it excellent wear resistance and self-lubricating properties. Therefore, MAX phase materials can become ideal reinforcements for preparing metal-based composite coating materials with excellent wear resistance and self-lubricating properties. In MAX phase-reinforced metal-based composite materials (copper-based, iron-based and nickel-based composite materials), it is generally observed that the A-site elements dissolve along the MAX phase (0001) crystal plane and diffuse to the metal interface, forming a new compound phase in situ, which is conducive to promoting the transformation of the bonding mode between the MAX phase and the metal matrix from mechanical bonding to metallurgical bonding, greatly improving the interfacial bonding strength, and giving the MAX phase-reinforced metal-based composite materials high strength, high modulus, and excellent ductility.

[0005] Therefore, it is of great practical value and scientific significance to develop a MAX phase metal-based composite coating with excellent wear resistance, self-lubricating properties and self-repairing properties to improve the tribological properties of the inner bore of the internal combustion engine cylinder body-piston ring and realize the remanufacturing and reuse of the inner bore of the cylinder body. Summary of the invention

[0006] The present invention is based on the mechanism that in the MAX phase where the A-position element is Al, the Al element can be desolvated along the MAX phase (0001) crystal plane and diffused to the metal matrix interface to form a new solid solution phase. By regulating the inner hole rotary plasma spraying process and the raw material powder ratio, the Ti2 An AlC-Fe based wear-resistant self-lubricating composite coating for the inner wall of an internal combustion engine cylinder body and a preparation method thereof.

[0007] The present invention provides a Ti 2 The AlC-Fe based wear-resistant self-lubricating coating comprises the following raw materials by mass percentage: 80% to 95% of Fe, 5% to 20% of Ti 2 AlC; wherein the Fe and Ti 2 The sum of the AlC components is 100%.

[0008] The present invention provides another Ti 2 The AlC-Fe based wear-resistant self-lubricating coating comprises the following components by mass percentage: 75% to 90% of Fe, 2% to 18% of Ti 2 AlC, 1% to 5% FexOy, 0.1% to 1% Ti 3 AlC 2 and 0.1% to 1% TiC; the Fe x O y For FeO, Fe 2 O 3 , Fe 3 O 4 One or more of the above; wherein the sum of the above components is 100%. It should be noted that this is because Fe in a part of the raw material powder will decompose into FexOy due to high temperature during the spraying process, and Ti in a part of the raw material powder will decompose into FexOy due to high temperature. 2 During the spraying process, AlC will decompose into Ti due to high temperature. 3 AlC 2 and TiC, so the Fe and Ti in the coating 2 The mass percentage of AlC will decrease, FexOy, Ti 3 AlC 2 The mass percentages of FexOy, TiC and other substances in the sprayed coating will increase. 3 AlC 2 and TiC are not impurities, but Fe and Ti 2 AlC decomposition products.

[0009] Furthermore, the particle size of the Fe is 15 μm to 45 μm, and the Ti 2 The particle size of AlC is 15 μm to 40 μm.

[0010] Furthermore, the microhardness of the wear-resistant self-lubricating coating is 400HV to 700HV.

[0011] Furthermore, the tensile bonding strength of the wear-resistant self-lubricating coating is 45MPa to 60MPa.

[0012] Furthermore, the friction coefficient of the wear-resistant self-lubricating coating is 0.2 to 0.3.

[0013] Furthermore, the thickness of the wear-resistant self-lubricating coating is 0.5 mm to 2 mm.

[0014] The present invention also provides the Ti 2 The preparation method of AlC-Fe based wear-resistant self-lubricating coating comprises the following steps: preparing raw material powders of each component according to a formula, placing the raw material powders of each component in a planetary ball mill for ball milling treatment until fully mixed, so as to obtain composite raw material powders; using carbon steel as a matrix, placing the matrix in a muffle furnace for preheating to 150° C.; placing the composite raw material powder in a powder feeder of an inner hole rotary plasma spraying device, fixing the preheated matrix on the inner hole rotary plasma spraying device, performing inner hole rotary plasma spraying treatment, and obtaining the Ti 2 AlC-Fe based wear-resistant self-lubricating coating; wherein the parameters of the spraying process include: a spray gun rotation speed of 120r / min, a spray gun vertical movement speed of 8mm / min, a distance between the spray gun and the inner wall of the cylinder body of 70mm, an argon gas flow rate of 70L / min to 100L / min, a hydrogen gas flow rate of 5L / min to 6.5L / min, a voltage of 100V to 120V, a current of 300A to 400A, and a powder feeding rate of 40g / min.

[0015] Furthermore, the ball milling treatment time is 8h to 12h.

[0016] Compared with the current prior art, the present invention has the following characteristics:

[0017] The present invention provides a Ti 2 AlC-Fe based wear-resistant self-lubricating coating and preparation method thereof, the wear-resistant self-lubricating coating directly uses existing raw material powder on the market as raw material, the raw material acquisition method is simple and low in cost, and the product has the characteristics of self-repair and reusability. 2 The preparation method of the AlC-Fe-based wear-resistant self-lubricating coating is simple and easy to operate by optimizing the inner hole rotary plasma spraying process and the raw material powder ratio, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] One or more embodiments are exemplarily described by pictures in the corresponding drawings, and these exemplifications do not constitute limitations on the embodiments. Unless otherwise stated, the pictures in the drawings do not constitute proportional limitations.

[0019] Figure 195wt.%Fe / 5wt.%Ti of Example 1 of the present invention 2 Scanning electron microscope image of AlC wear-resistant self-lubricating coating;

[0020] Figure 2 90wt.%Fe / 10wt.%Ti of Example 2 of the present invention 2 Scanning electron microscope image of AlC wear-resistant self-lubricating coating;

[0021] Figure 3 85wt.%Fe / 15wt.%Ti of Example 3 of the present invention 2 Scanning electron microscope image of AlC wear-resistant self-lubricating coating;

[0022] Figure 4 80wt.%Fe / 20wt.%Ti of Example 4 of the present invention 2 Scanning electron microscope image of AlC wear-resistant self-lubricating coating. DETAILED DESCRIPTION

[0023] The inventors found that in order to meet the requirements of good integration with the cast iron cylinder block of heavy-duty automobile internal combustion engines, Fe-based coatings that are homogeneous with the cylinder block of heavy-duty automobile internal combustion engines are the first choice. However, the mechanical properties of pure Fe-based coatings are extremely poor and do not have wear-resistant and self-lubricating properties, so it is necessary to design a second-phase reinforced Fe-based composite coating. The new ternary layered MAX phase ceramic is a good damage tolerance ceramic material that combines high strength and high toughness with excellent metal-like electrical conductivity. Typical materials include Ti 3 SiC 2 、Ti 2 AlC、Ti 3 (SiAl)C 2 Solid solution and Cr 2 AlC, its density is 4-5g / cm 3 , Young's modulus is 280~340GPa, and room temperature fracture toughness is 6.0~7.88MPa·m 1 / 2 In addition, the new ternary MAX phase ceramics have the comprehensive advantages of excellent wear resistance, self-lubrication, resistance to thermal shock, resistance to thermal cycling, high temperature self-healing repair, oxidation resistance and good wettability with the metal matrix interface. How to prepare a Ti2AlC reinforced Fe-based coating that can replace the traditional cast iron cylinder liner by optimizing the inner hole rotary plasma spraying process and the raw material powder ratio has become a key issue in the development of this new Ti 2 Key points of AlC-Fe based wear-resistant self-lubricating coating.

[0024] The present invention provides a Ti 2 The AlC-Fe based wear-resistant self-lubricating coating comprises the following raw materials by mass percentage: 80% to 95% of Fe, 5% to 20% of Ti2 AlC; wherein the Fe and Ti 2 The sum of the AlC components is 100%.

[0025] It should be noted that Ti 2 AlC can also be replaced by other MAX phase ceramics, including but not limited to Ti 3 AlC 2 、Ti 3 SiC 2 Cr 2 AlC and Mo 2 One or more of AlB. The Ti listed above 2 AlC、Ti 3 AlC 2 、Ti 3 SiC 2 Cr 2 AlC and Mo 2 AlB is the same type of chemical substance, so it can be used as the raw material to prepare a wear-resistant self-lubricating coating with the same performance.

[0026] The present invention also provides a Ti 2 The AlC-Fe based wear-resistant self-lubricating coating comprises the following components by mass percentage: 75% to 90% of Fe, 2% to 18% of Ti 2 AlC, 1% to 5% FexOy, 0.1% to 1% Ti 3 AlC 2 and 0.1% to 1% TiC; the Fe x O y For FeO, Fe 2 O 3 , Fe 3 O 4 One or more of the above; wherein the sum of the above components is 100%.

[0027] Wherein, the particle size of Fe is 15 μm to 45 μm, and the particle size of Ti is 2 The particle size of AlC is 15 μm to 40 μm.

[0028] The present invention also provides the Ti 2 A method for preparing an AlC-Fe based wear-resistant self-lubricating coating, the method comprising the following steps:

[0029] S1. Prepare raw material powders of each component according to the formula, place the raw material powders of each component in a planetary ball mill for ball milling until fully mixed, and obtain composite raw material powders;

[0030] S2, using carbon steel as a substrate, placing the substrate in a muffle furnace and preheating it to 150° C.;

[0031] S3, placing the composite raw material powder in a powder feeder of an inner hole rotary plasma spraying device, fixing the preheated substrate on the inner hole rotary plasma spraying device, and performing inner hole rotary plasma spraying treatment to obtain the Ti 2 AlC-Fe based wear-resistant self-lubricating coating;

[0032] Among them, the parameters of the spraying process include: spray gun rotation speed 120r / min, spray gun vertical movement speed 8mm / min, spray gun and cylinder inner wall distance 70mm, argon gas flow rate 70L / min~100L / min, hydrogen gas flow rate 5L / min~6.5L / min, voltage 100V~120V, current 300A~400A, powder feeding rate 40g / min.

[0033] It should be noted that, for the formula of the first wear-resistant self-lubricating coating provided in the present invention, the raw material powders of the above components are specifically Fe and Ti 2 AlC; and for the first wear-resistant self-lubricating coating formulation provided in the present invention, the raw material powders of the above components are specifically Fe, Ti 2 AlC, FexOy, Ti 3 AlC 2 and TiC.

[0034] The present invention is described in detail below in conjunction with specific implementation modes.

[0035] Example 1

[0036] Embodiment 1 provides a Ti 2 AlC-Fe based wear-resistant self-lubricating coating and preparation method thereof, the preparation method comprising:

[0037] According to the mass percentage of the raw material powder of the wear-resistant self-lubricating coating: Fe: 95%, Ti 2 AlC: 5%, the sum of the two components is 100%, weigh the required Fe and Ti 2 AlC;

[0038] The two raw material powders are placed in a planetary ball mill and ball milled for 8 to 12 hours to achieve full mixing;

[0039] The carbon steel substrate was placed in a muffle furnace and preheated to 150°C;

[0040] The composite raw material powder is placed on the powder feeder of the inner hole rotary plasma spraying equipment, the preheated carbon steel substrate is fixed on the inner hole rotary plasma spraying equipment by a clamp, and the plasma spraying parameters are used, and then the inner hole rotary plasma spraying wear-resistant self-lubricating coating is prepared, and finally the wear-resistant self-lubricating coating is obtained. Figure 1 As shown, the Ti inside the coating 2 AlC presents a layered morphology and is dispersed in Fe. The wear-resistant self-lubricating coating has a microhardness of 400±50HV and a coating bonding strength of 60±5MPa.

[0041] Example 2

[0042] Embodiment 2 provides a Ti 2 AlC-Fe based wear-resistant self-lubricating coating and preparation method thereof, the preparation method comprising:

[0043] According to the mass percentage of the raw material powder of the wear-resistant self-lubricating coating: Fe: 90%, Ti 2 AlC: 10%, the sum of the two components is 100%, weigh the required Fe and Ti 2 AlC;

[0044] The two raw material powders are placed in a planetary ball mill and ball milled for 8 to 12 hours to achieve full mixing;

[0045] The carbon steel substrate was placed in a muffle furnace and preheated to 150°C;

[0046] The composite raw material powder is placed on the powder feeder of the inner hole rotary plasma spraying equipment, the preheated carbon steel substrate is fixed on the inner hole rotary plasma spraying equipment by a clamp, and the plasma spraying parameters are used, and then the inner hole rotary plasma spraying wear-resistant self-lubricating coating is prepared, and finally the wear-resistant self-lubricating coating is obtained. Figure 2 As shown, the Ti inside the coating 2 AlC presents a layered morphology and is dispersed in Fe. The wear-resistant self-lubricating coating has a microhardness of 500±50HV and a coating bonding strength of 55±5MPa.

[0047] Example 3

[0048] Embodiment 3 provides a Ti 2 AlC-Fe based wear-resistant self-lubricating coating and preparation method thereof, the preparation method comprising:

[0049] According to the mass percentage of the raw material powder of the wear-resistant self-lubricating coating: Fe: 85%, Ti 2 AlC: 15%, the sum of the two components is 100%, weigh the required Fe and Ti 2 AlC;

[0050] The two raw material powders are placed in a planetary ball mill and ball milled for 8 to 12 hours to achieve full mixing;

[0051] The carbon steel substrate was placed in a muffle furnace and preheated to 150°C;

[0052] The composite raw material powder is placed on the powder feeder of the inner hole rotary plasma spraying equipment, the preheated carbon steel substrate is fixed on the inner hole rotary plasma spraying equipment by a clamp, and the plasma spraying parameters are used, and then the inner hole rotary plasma spraying wear-resistant self-lubricating coating is prepared, and finally the wear-resistant self-lubricating coating is obtained. Figure 3 As shown, the Ti inside the coating 2 AlC presents a layered morphology and is dispersed in Fe. The wear-resistant self-lubricating coating has a microhardness of 600±50HV and a coating bonding strength of 50±5MPa.

[0053] Example 4

[0054] Example 4 provides a Ti 2 AlC-Fe based wear-resistant self-lubricating coating and preparation method thereof, the preparation method comprising:

[0055] According to the mass percentage of the raw material powder of the wear-resistant self-lubricating coating: Fe: 80%, Ti 2 AlC: 20%, the sum of the two components is 100%, weigh the required Fe and Ti 2 AlC;

[0056] The two raw material powders are placed in a planetary ball mill and ball milled for 8 to 12 hours to achieve full mixing;

[0057] The carbon steel substrate was placed in a muffle furnace and preheated to 150°C;

[0058] The composite raw material powder is placed on the powder feeder of the inner hole rotary plasma spraying equipment, the preheated carbon steel substrate is fixed on the inner hole rotary plasma spraying equipment by a clamp, and the plasma spraying parameters are used, and then the inner hole rotary plasma spraying wear-resistant self-lubricating coating is prepared, and finally the wear-resistant self-lubricating coating is obtained. Figure 4 As shown, the Ti inside the coating 2 AlC presents a layered morphology and is dispersed in Fe. The wear-resistant self-lubricating coating has a microhardness of 700±50HV and a coating bonding strength of 45±5MPa.

[0059] Those skilled in the art can understand that the above-mentioned embodiments are specific examples for implementing the present application, and in practical applications, various changes can be made to them in form and detail without departing from the spirit and scope of the present application. Any person skilled in the art can make their own changes and modifications without departing from the spirit and scope of the present application, so the scope of protection of the present application shall be based on the scope defined in the claims.

Claims

1. A Ti2AlC-Fe based wear-resistant self-lubricating coating, characterized in that: The wear-resistant self-lubricating coating comprises the following raw materials in terms of mass percentage: 80% to 95% of Fe, 5% to 20% of Ti2AlC; wherein the sum of the components of Fe and Ti2AlC is 100%; The particle size of Fe is 15 μm to 45 μm, and the particle size of Ti2AlC is 15 μm to 40 μm; the thickness of the wear-resistant self-lubricating coating is 0.5 mm to 2 mm; The preparation method of the wear-resistant self-lubricating coating comprises the following steps: S1. Prepare raw material powders of each component according to the formula, place the raw material powders of each component in a planetary ball mill for ball milling until fully mixed, and obtain composite raw material powders; S2, using carbon steel as a substrate, placing the substrate in a muffle furnace and preheating it to 150° C.; S3, placing the composite raw material powder in a powder feeder of an inner hole rotary plasma spraying device, fixing the preheated substrate on the inner hole rotary plasma spraying device, and performing inner hole rotary plasma spraying treatment to obtain the Ti2AlC-Fe based wear-resistant self-lubricating coating; Among them, the parameters of the spraying process include: spray gun rotation speed 120r / min, spray gun vertical movement speed 8mm / min, spray gun and cylinder inner wall distance 70mm, argon gas flow rate 70L / min~100L / min, hydrogen gas flow rate 5L / min~6.5L / min, voltage 100V~120V, current 300A~400A, powder feeding rate 40g / min.

2. A Ti2AlC-Fe based wear-resistant self-lubricating coating, characterized in that: The wear-resistant self-lubricating coating comprises the following components by mass percentage: 75% to 90% of Fe, 2% to 18% of Ti2AlC, 1% to 5% of Fe x O y , 0.1% to 1% Ti3AlC2 and 0.1% to 1% TiC; the Fe x O y It is one or more of FeO, Fe2O3, and Fe3O4; wherein the sum of the components is 100%; The particle size of Fe is 15 μm to 45 μm, and the particle size of Ti2AlC is 15 μm to 40 μm; the thickness of the wear-resistant self-lubricating coating is 0.5 mm to 2 mm; The preparation method of the wear-resistant self-lubricating coating comprises the following steps: S1. Prepare raw material powders of each component according to the formula, place the raw material powders of each component in a planetary ball mill for ball milling until fully mixed, and obtain composite raw material powders; S2, using carbon steel as a substrate, placing the substrate in a muffle furnace and preheating it to 150° C.; S3, placing the composite raw material powder in a powder feeder of an inner hole rotary plasma spraying device, fixing the preheated substrate on the inner hole rotary plasma spraying device, and performing inner hole rotary plasma spraying treatment to obtain the Ti2AlC-Fe based wear-resistant self-lubricating coating; Among them, the parameters of the spraying process include: spray gun rotation speed 120r / min, spray gun vertical movement speed 8mm / min, spray gun and cylinder inner wall distance 70mm, argon gas flow rate 70L / min~100L / min, hydrogen gas flow rate 5L / min~6.5L / min, voltage 100V~120V, current 300A~400A, powder feeding rate 40g / min.

3. The Ti2AlC-Fe based wear-resistant self-lubricating coating according to claim 1 or 2, characterized in that: The microhardness of the wear-resistant self-lubricating coating is 400HV to 700HV.

4. The Ti2AlC-Fe based wear-resistant self-lubricating coating according to claim 1 or 2, characterized in that: The tensile bonding strength of the wear-resistant self-lubricating coating is 45MPa to 60MPa.

5. The Ti2AlC-Fe based wear-resistant self-lubricating coating according to claim 1 or 2, characterized in that: The friction coefficient of the wear-resistant self-lubricating coating is 0.2-0.

3.

6. The Ti2AlC-Fe based wear-resistant self-lubricating coating according to claim 1 or 2, characterized in that: The ball milling treatment time is 8h to 12h.

Citation Information

Patent Citations

  • In-situ preparation of wear-resistant self-lubricating coating on surface of titanium alloy by laser cladding

    CN104480460A

  • Plasma spray gradient wear-resistant plate and preparation method and application thereof

    CN106367706A

  • Gas turbine part and method for manufacturing such gas turbine part

    CN106947902A

  • Laser cladding in-situ grown high-temperature self-lubricating anti-wear composite coating and preparation method thereof