A heat-treatment-free 1100MPa-grade hot-rolled steel plate for automobile upper body and production method thereof
By optimizing chemical composition and process flow, a high-strength, easy-to-cut and corrosion-resistant 1100MPa-grade hot-rolled steel plate was prepared, which solved the problems of high cost and complex process in the existing technology, and achieved high performance to meet the needs of the automotive industry. Steel plate production.
Patent Information
- Application Number
- CN202310785527.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-29
AI Technical Summary
The prior art cannot effectively produce 1100MPa grade hot-rolled steel plates that meet the automotive industry's requirements for high strength, low cost, easy cutting and corrosion resistance, and lack heat-free treatment processes.
By optimizing the chemical composition design, the reasonable proportion of elements such as C, Si, Mn, Ti, V, Cr, B, Mo, Cu, Ni, Bi, Sb, rare earths, etc. are adopted, combined with LF+RH refining, electromagnetic stirring continuous casting, Heating, hot rolling, rapid cooling and hood-injection and slow cooling process were used to prepare martensite tissue hot rolled steel plates with yield strength ≥950MPa, tensile strength ≥1100MPa, and transverse elongation A50≥22%.
It achieves high strength, high elongation, good machinability and corrosion resistance, is suitable for steel for dump trucks and modified trucks, and avoids high cost and complex processes in traditional heat treatment.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal materials, and particularly relates to a heat-treatment-free 1100MPa-grade hot-rolled steel plate for automobile upper parts and a production method thereof. Background Art
[0002] The automotive industry is a major user of steel products, and the research and development and application of steel products are closely related to the development trend of the automotive industry. In today's society, the automotive industry is developing in the direction of low cost, high reinforcement, green environmental protection, and high safety. The demand for hot-rolled high-strength steel is increasing. The specific requirements are: steel plate yield strength ≥ 950MPa, tensile strength ≥ 1100MPa, transverse elongation A 50 ≥22%, Brinell hardness HBW ≥323, thickness ≥5mm, -40℃ impact energy greater than 65J, and the structure is martensite.
[0003] The Chinese patent application with publication number CN111254351A discloses a high-performance hot-rolled wear-resistant steel sheet and its production method, which uses a common C-Mn component system to design and add a certain amount of Nb, Ti, Cr and other elements, and improves the strength through solid solution strengthening of carbon and manganese elements and fine grain strengthening and precipitation strengthening of niobium and titanium elements. The elongation after fracture of the steel sheet is ≥14%, which does not meet the requirements of difficult-to-form steel for automobile upper parts, and has defects such as high cost, lack of machinability and corrosion resistance. The Chinese invention patent with publication number CN110964985A discloses a molybdenum-free low-alloy wear-resistant steel sheet and its production method, which uses vanadium to inhibit austenite recrystallization and grain growth, and can obtain finer ferrite crystals after phase transformation, improve the strength of the steel sheet and improve the toughness of the steel sheet. The production process requires quenching and tempering and other treatment processes, and the process is relatively complicated. The elongation after fracture of the steel sheet is ≥12%, which does not meet the requirements of difficult-to-form steel for automobile upper parts, and does not have machinability and corrosion resistance. Up to now, there has been no report on the relevant research on the production method of 1100MPa grade hot-rolled steel plates for automobile body without heat treatment. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a heat-treatment-free 1100MPa-grade hot-rolled steel plate for automobile upper body and a production method. The heat-treatment-free 1100MPa-grade hot-rolled steel plate for automobile upper body produced by the present invention has a yield strength of ≥950MPa, a tensile strength of ≥1100MPa, and a transverse elongation A 50 ≥22%, Brinell hardness HBW ≥323, thickness ≥2mm, the impact energy of the finished steel plate with a thickness of 6.0-10.0mm at -40℃ is greater than 65J, and the structure is martensite.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] The present invention provides a heat-treatment-free 1100MPa-grade hot-rolled steel plate for automobile upper parts. The chemical composition and mass percentage of the hot-rolled steel plate are as follows: C: 0.09%-0.16%, Si: 0.10%-0.40%, Mn: 1.00%-1.55%, S: 0.009%-0.022%, Al: 0.020%-0.062%, Ti: 0.020%-0.055%, V: 0.020%-0.065%, Cr: 0.10%- 0.25%, B: 0.0015%-0.0033%, Mo: 0.10%-0.16%, Cu: 0.25%-0.55%, Ni: 0.10%-0.20%, Bi: 0.010%-0.055%, Sb: 0.035%-0.060%, rare earth: 0.030%-0.053%, Ca: 0.004%-0.018%, P≤0.018%, N≤0.005%, the balance is Fe and unavoidable impurities.
[0007] Based on the above technical solution, further, the rare earth is La+Ce.
[0008] The main mechanism of action of the chemical composition of the heat-treatment-free 1100MPa grade hot-rolled steel sheet for automobile upper body of the present invention is:
[0009] C: Carbon is mainly used to form the required amount of martensite and ensure the strength of steel. It is also the most important solid solution strengthening element in steel. The increase of carbon element is beneficial to increase the hardenability of steel. The optimal range of carbon in the present invention is 0.09%-0.16%.
[0010] Si: Silicon is a solid solution strengthening element, which can improve the strength of the steel plate through solid solution strengthening. It also has the effect of improving the hardenability of the steel plate and promoting the enrichment of carbon into the untransformed austenite, thereby improving the stability of the austenite. The silicon content in the present invention is 0.10%-0.40%.
[0011] Mn: Manganese can form substitutional solid solution in steel, play a strong solid solution strengthening role, and increase the yield strength and tensile strength linearly. The content of this element increases the strength of steel within a certain range without reducing the plasticity and toughness of steel. It is also an austenite stabilizing element, and can also improve the hardenability of steel and significantly delay the pearlite transformation. However, if the manganese content is too high, the carbon equivalent of steel will increase, and the uniformity of the steel plate structure will deteriorate during the smelting and hot rolling process, which is easy to cause serious banded structure defects in the structure. Therefore, the manganese content is selected to be 1.00%-1.55%.
[0012] P: Phosphorus can increase the formation temperature of α phase, expand the temperature range of α phase, delay the formation of cementite, and increase the stability of austenite; at the same time, phosphorus significantly changes the morphology of martensite islands, making the size of martensite islands smaller and more evenly distributed. However, excessive phosphorus content will deteriorate the processability of steel plates. In order to obtain a higher elongation, the phosphorus content is selected to be ≤0.018%.
[0013] S: Sulfur can form sulfide inclusions such as MnS in steel. Such inclusions can interrupt the continuity of the base metal, causing the chips to form a small and short curling radius during cutting, which is easy to remove, reducing tool wear, reducing the roughness of the processed surface, and increasing the tool life, achieving easy cutting. Generally, the machinability of steel increases with the increase of sulfur content in the steel. However, when the sulfur content in the steel is too high, it will cause hot brittleness, making it difficult to hot process the steel and deteriorating the mechanical properties of the steel. Therefore, the sulfur content is controlled to be 0.009%-0.022% in the present invention.
[0014] Al: Al is a commonly used deoxidizer in steel. It plays a role in deoxidation and nitrogen determination during the smelting process and can effectively improve the anti-oxidation performance of the steel plate. Adding a certain amount of Al to the steel can form AlN precipitation, which plays a certain role in refining the grains. Therefore, in the present invention, the Al content is limited to 0.020%-0.062%.
[0015] Ti: Titanium can effectively delay the recrystallization of deformed austenite, prevent the growth of austenite grains, increase the austenite recrystallization temperature, refine the grains, and improve the strength and toughness of steel. Moreover, Ti is a strong carbon and nitride forming element, which can combine with carbon and nitrogen to form stable and fine carbon and nitride, playing a significant precipitation strengthening role, and can also inhibit the precipitation of BN, avoiding the reduction of strength caused by the precipitation of B. Therefore, the titanium content of the present invention is selected to be 0.020%-0.055%.
[0016] V: Vanadium has significant precipitation strengthening and fine grain strengthening effects. The effect of vanadium is mainly achieved by forming precipitates with carbon and nitrogen. In particular, the precipitation of VN formed with nitrogen can greatly improve the strength of the steel plate, and can inhibit the precipitation of BN, avoiding the reduction of strength caused by the precipitation of B. In addition, the addition of V can also be combined with H to improve the delayed fracture resistance of the steel plate. In the present invention, the addition amount of V is 0.020%-0.065%.
[0017] Cr: It is a carbide-forming element that can delay pearlite transformation and improve the hardenability of steel. It is conducive to the formation of martensite structure, refines the structure, and has a strengthening effect. Too high chromium content will make the processing and formability of the material worse. The principle of selecting the chromium content is to promote the formation of martensite, so the chromium content of the present invention is selected in the range of 0.10%-0.25%.
[0018] B: Boron can significantly improve the hardenability of steel and is beneficial to the formation of martensite structure. When the B content is higher than 0.0050%, the excess B forms B compounds with N in the steel, reducing the performance of the steel plate. Therefore, the boron content of the present invention is in the range of 0.0015%-0.0033%.
[0019] Mo: Mo is a carbide-forming element that can improve the strength and toughness of steel plates. Mo can significantly improve austenite stability, increase the hardenability of steel, and is beneficial to the formation of martensite structure. Therefore, the Mo content of the present invention is selected to be 0.10%-0.16%.
[0020] Cu: Copper can expand the austenite phase, improve the weather resistance of steel, improve the weldability of steel, and effectively improve the corrosion resistance of steel. However, when the Cu content is high, it causes hot brittleness and deteriorates the surface performance of the steel plate. In addition, at a certain Cu content, it is beneficial to the strength and hot workability of the steel plate, effectively reduces the tendency of hot rolling edge cracking of the steel plate, and significantly improves the surface quality of the steel plate. Cu also has the effect of reducing work hardening and improving the plasticity of the steel plate. Therefore, the copper content of the present invention is selected between 0.25% and 0.55%.
[0021] Ni: Nickel has no adverse effect on the hardenability and toughness of the welding heat affected zone of steel, and can improve the corrosion resistance and hardenability of steel, which is beneficial to the formation of martensitic structure. Therefore, the Ni content in the steel of the present invention is selected to be 0.10%-0.20%.
[0022] Bi: Bismuth is mainly distributed in the grain boundaries and inside the grains in steel, which improves the strength of the steel plate, reduces the diffusion rate of carbon, oxygen and other elements on the grain boundaries, reduces decarburization and oxidation, and improves the surface and mechanical properties of the steel plate. Therefore, the present invention limits the Bi content to 0.010%-0.055%.
[0023] Sb: Antimony is mainly distributed in the grain boundaries and grain interiors in steel, which improves the strength of the steel plate, reduces the diffusion rate of elements such as carbon and oxygen on the grain boundaries, reduces decarburization and oxidation, and improves the surface and mechanical properties of the steel plate. The addition of antimony will cause a uniform and dense oxide film (rich in Sb, Cu, Cr and other elements) to form on the surface of the steel plate matrix, which can effectively prevent air moisture and oxygen from continuing to enter the matrix to form a corrosive internal environment, improve the corrosion resistance of the matrix, and enhance the corrosion resistance of the steel plate. If the Sb content is too low, the passivation film will be unevenly dispersed and the overall anti-corrosion effect will not be achieved; when it exceeds the design upper limit, it has an anti-corrosion effect, but significantly reduces the hot working performance. Therefore, the present invention limits the Sb content to 0.035% to 0.060%.
[0024] Rare earth: Rare earth RE has strong deoxidation and desulfurization capabilities. The spherical sulfide or sulfur oxide formed replaces the long strip manganese sulfide inclusions, which can improve the plasticity and anisotropy of the steel plate. Rare earth can improve the fatigue performance of the steel plate, improve the welding performance of the steel plate, and improve the cold forming performance of the steel plate. Rare earth has a strong affinity with other impurity elements in steel, which can reduce the content of sulfur, oxygen, phosphorus, hydrogen and other elements in the steel and eliminate their harmful effects. Therefore, the present invention limits the content of rare earth RE to 0.030%-0.053%.
[0025] Ca: Calcium can change the form of steel sulfide (MnS), prevent the formation of long strips of MnS inclusions, and improve the plasticity, toughness and fatigue properties of the steel plate. Therefore, the present invention controls the Ca content to 0.004-0.018%.
[0026] N: Nitrogen is an impurity element in the present invention, and the smaller its content, the better. For B-containing steel, the lower the N content, the better. However, too low a content will lead to production difficulties and increase costs. Therefore, the N content in the present invention is ≤0.005%.
[0027] Based on the above technical solution, further, the hot-rolled steel plate has a structure of martensite, a yield strength of ≥950MPa, a tensile strength of ≥1100MPa, and a transverse elongation A 50 ≥22%, Brinell hardness HBW≥323.
[0028] The present invention also provides a method for producing the above-mentioned heat-treatment-free 1100MPa grade hot-rolled steel plate for automobile upper body, which mainly includes smelting, refining, continuous casting, heating, hot rolling, rapid cooling, coiling and hood slow cooling process; wherein,
[0029] During the heating process, the heating temperature is 1310-1350°C and the holding time is 166-192min; appropriate heating temperature and suitable holding time can make the alloy elements in the slab completely dissolved, the slab composition uniform, and play a role in controlling the original austenite grain size.
[0030] The hot rolling process is divided into two stages: rough rolling and finishing rolling. The rough rolling adopts a 3+3 rolling process (R1 adopts 3 passes, R2 adopts 3 passes), with a total of 6 passes, and the rough rolling outlet temperature is 1115-1180°C. The finishing rolling adopts 7-stand continuous rolling, the finishing rolling inlet temperature is 1080-1115°C, and the final rolling temperature is 845-955°C.
[0031] The cooling rate of the rapid cooling process is 165-185°C / s.
[0032] Based on the above technical solution, further, the refining adopts LF+RH process to control H≤0.0002%, O≤0.0015%, and calcium treatment is performed during the refining process to ensure w(Ca) / w(Al)=0.09-0.14.
[0033] Based on the above technical solution, electromagnetic stirring and light reduction technology are further used in the continuous casting process, the billet pulling speed is ≤1.1m / min, and the billets are stacked and slowly cooled after they come off the line.
[0034] Based on the above technical solution, further, the heating process is always dynamically controlled in a slightly positive pressure state, and the positive pressure value is controlled at 3 to 15Pa.
[0035] Based on the above technical solution, further, during the hot rolling process, the intermediate billet thickness is 45 to 68 mm, and an insulation cover is used to keep the intermediate billet warm before entering the finishing mill to reduce the temperature drop of the intermediate billet on the delay roller and the temperature difference between the head and tail and the plate width direction.
[0036] Based on the above technical solution, high-pressure water descaling is further performed before finish rolling.
[0037] Based on the above technical solution, further, the coiling temperature in the coiling process is 75-112°C. The purpose of ultra-fast cooling to the coiling temperature is to cool to the martensite zone at a cooling rate greater than the critical cooling rate for the transformation of pearlite and bainite, avoiding the pearlite and bainite formation zone, while inhibiting grain growth, the martensite content is also guaranteed, thereby refining the martensite grains.
[0038] Based on the above technical solution, further, the slow cooling cover temperature is 150-255°C, and the insulation time is 30-60min.
[0039] Based on the above technical solution, further, after the slow cooling is completed, the steel coil is taken out and air-cooled to room temperature.
[0040] The beneficial effects of the present invention compared with the prior art are as follows:
[0041] The present invention first optimizes the chemical composition of the hot-rolled high-strength steel, and then adopts the process of heating, hot rolling, rapid cooling, coiling and slow cooling in a hood according to the chemical composition of the hot-rolled high-strength steel. The hot-rolled high-strength steel has excellent mechanical properties, yield strength ≥950MPa, tensile strength ≥1100MPa, transverse elongation A 50 ≥22%, Brinell hardness HBW ≥323, thickness ≥2mm, the finished steel plate with a thickness of 6.0-10.0mm has an impact energy of more than 65J at -40℃, and the organization is 100% martensite, which is fully suitable for manufacturing steel for dump trucks and modified vehicles. DETAILED DESCRIPTION
[0042] The present invention is described in detail below with reference to the embodiments, but the embodiments of the present invention are not limited thereto. Obviously, the embodiments described below are only partial embodiments of the present invention. For those skilled in the art, other similar embodiments obtained without creative labor all fall within the protection scope of the present invention.
[0043] Examples 1-6
[0044] This embodiment provides a method for producing a heat-treatment-free 1100MPa grade hot-rolled steel plate for automobile upper parts. The chemical composition and weight percentage of the hot-rolled steel plate in the embodiment are shown in Table 1;
[0045] Table 1 Chemical composition of hot-rolled steel sheets of the present invention (wt, %)
[0046]
[0047] The following steps are involved:
[0048] (1) Smelting and refining: LF+RH process is adopted to strictly control the H and O contents, H≤0.0002%, O≤0.0015%, and calcium treatment is performed in the refining process to ensure w(Ca) / w(Al)=0.09-0.14;
[0049] (2) Continuous casting: Electromagnetic stirring and light pressure reduction technology are used in the continuous casting process, and the billet pulling speed is ≤1.1m / min. The billets are stacked and slowly cooled after they come off the line;
[0050] (3) Heating: The continuous casting slab is sent to a walking beam heating furnace for heating. The heating temperature and holding time parameters are shown in Table 2. The furnace pressure is always dynamically controlled in a slightly positive pressure state, and the positive pressure value is controlled at 3-15 Pa to reduce oxidation and burning.
[0051] (4) Hot rolling: Hot rolling is divided into two stages: rough rolling and finishing rolling. Rough rolling adopts a 3+3 rolling process (R1 adopts 3 passes, R2 adopts 3 passes), with a total of 6 passes. The rough rolling outlet temperature is the parameter shown in Table 2. The intermediate billet thickness is 45-68 mm, and the width is 1510-1850 mm. The intermediate billet is kept warm by a heat preservation cover before entering the hot rolling and finishing mill to reduce the temperature drop of the intermediate billet on the delay roller and the temperature difference between the head and tail and the plate width direction. Finishing rolling is a 7-stand continuous rolling. High-pressure water descaling is performed before finishing rolling. The parameters of finishing rolling inlet temperature and final rolling temperature are shown in Table 2.
[0052] (5) Rapid cooling: After final rolling, ultra-fast cooling mode is adopted. The ultra-fast cooling rate parameters are shown in Table 2;
[0053] (6) Coiling: Coil the steel plate when it is cooled to the coiling temperature (see Table 2);
[0054] (7) Slow cooling in the hood: After coiling, the steel coil is immediately placed in a heated slow cooling hood. The temperature and insulation time of the slow cooling hood are shown in Table 2. The steel coil is taken out and air cooled to room temperature.
[0055] Table 2 Production process parameters of Examples 1-6 of the present invention
[0056]
[0057] The convexity control accuracy of the steel plate produced by the above production method is ±40μm, the flatness is controlled within 18I, the thickness control accuracy is ±40μm, the finished steel plate thickness, the steel plate performance and the tissue volume percentage are shown in Table 3.
[0058] Table 3 Mechanical properties parameters and tissue volume percentage of the steel plates of Examples 1-6 of the present invention
[0059]
[0060] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A heat-treatment-free 1100MPa grade hot-rolled steel plate for automobile body, It is characterized in that The chemical composition and mass percentage of the hot-rolled steel sheet are as follows: C: 0.09%-0.16%, Si: 0.10%-0.40%, Mn: 1.00%-1.55%, S: 0.009%-0.022%, Al: 0.020%-0.062%, Ti: 0.020%-0.055%, V: 0.020%-0.065%, Cr: 0.10%-0.25%, B: 0.0015 %-0.0033%, Mo: 0.10%-0.16%, Cu: 0.25%-0.55%, Ni: 0.10%-0.20%, Bi: 0.010%-0.055%, Sb: 0.035%-0.060%, rare earth: 0.030%-0.053%, Ca: 0.004%-0.018%, P≤0.018%, N≤0.005%, the balance is Fe and unavoidable impurities; The rare earth is La+Ce; The hot-rolled steel sheet has a martensite structure, a yield strength of ≥950MPa, a tensile strength of ≥1100MPa, and a transverse elongation of A 50 ≥22%, Brinell hardness HBW≥323; The production method of the heat-treatment-free 1100MPa grade hot-rolled steel plate for automobile upper body comprises the process of smelting, refining, continuous casting, heating, hot rolling, rapid cooling, coiling and hood slow cooling; wherein, During the heating process, the heating temperature is 1310-1350°C and the holding time is 166-192min; The hot rolling process is divided into two stages: rough rolling and finishing rolling. The rough rolling outlet temperature is 1115-1180°C. The finishing rolling adopts continuous rolling, the finishing rolling inlet temperature is 1080-1115°C, and the final rolling temperature is 845-955°C. The cooling rate of the rapid cooling process is ≥165℃ / s; The coiling temperature during the coiling process is ≤112℃; After coiling, it immediately enters the heated slow cooling hood, the slow cooling hood temperature is 150-255℃, and the insulation time is 30-60min.
2. The heat-treatment-free 1100MPa grade hot-rolled steel sheet for automobile body according to claim 1, It is characterized in that The LF+RH process is used for refining, and H is controlled to be ≤ 0.0002%, and O is controlled to be ≤ 0.0015%. Calcium treatment is performed during the refining process to ensure that w(Ca) / w(Al)=0.09-0.
14.
3. The heat-treatment-free 1100MPa grade hot-rolled steel sheet for automobile body according to claim 1, It is characterized in that Electromagnetic stirring and light reduction technology are used in the continuous casting process. The billet pulling speed is ≤1.1m / min. The billets are stacked and slowly cooled after they come off the line.
4. The heat-treatment-free 1100MPa grade hot-rolled steel sheet for automobile body according to claim 1, It is characterized in that During the heating process, the system is always dynamically controlled in a slightly positive pressure state, and the positive pressure value is controlled within a range of 3 to 15 Pa.
5. The heat-treatment-free 1100MPa grade hot-rolled steel sheet for automobile body according to claim 1, It is characterized in that During the hot rolling process, the thickness of the intermediate billet is 45 to 68 mm. A heat preservation cover is used to keep the intermediate billet warm before it enters the finishing mill. High-pressure water is used to remove scale before finishing rolling.