A titanium oxide ceramic with high mechanical strength and a preparation method thereof
By using raw materials such as anatase-type titanium oxide powder and specific process steps, high mechanical strength titanium oxide ceramics are prepared, which solves the balance problem between electrochemical properties and mechanical strength of existing materials and significantly improves zinc The electrochemical properties and corrosion resistance of nickel batteries extend the service life of the battery.
Patent Information
- Application Number
- CN202311012056.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-11
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-08-11
AI Technical Summary
Existing titanium oxide conductive ceramic materials are difficult to balance electrochemical performance and mechanical strength, and cannot effectively improve the cycle life and chemical corrosion resistance of zinc-nickel batteries.
Using raw materials such as anatase titanium oxide powder, butyl titanate, silane coupling agent, polyvinyl alcohol microspheres, N,N'-methylenebisacrylamide and diethylenetriamine, through specific process steps Such as dispersion, stirring, calcination and sonication, high mechanical strength titanium oxide ceramics are formed to enhance their conductivity and corrosion resistance.
The prepared titanium oxide ceramic has high conductivity, stability and biocompatibility, forming a large pore and hard Magnéli phase titanium oxide powder, which significantly improves the electrochemical reaction activity and production efficiency of zinc-nickel batteries. Extends the battery's cycle life.
Smart Images

Figure CN116969757B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium oxide, and in particular to a titanium oxide ceramic with high mechanical strength and a preparation method thereof. Background Art
[0002] Chemical power sources have many advantages, such as strong mobility, almost no pollution to the environment, and relatively high energy efficiency. Therefore, with the rapid development of science and technology today, the development of chemical power sources has received great attention. Although people have conducted in-depth research on zinc-nickel battery systems, there are still some problems that restrict the further development of zinc-nickel batteries.
[0003] At present, during the charge and discharge cycle of zinc-nickel batteries, the uneven distribution of current density causes deformation and corrosion of the zinc negative electrode, which seriously affects the cycle life of zinc-nickel batteries. Zinc-nickel batteries are in urgent need of a material that is resistant to chemical corrosion, has good conductivity, and is electrochemically stable to effectively improve their performance.
[0004] Titanium oxide materials have excellent electrochemical properties, with conductivity up to 1500S / cm, which is much higher than graphite materials. They have strong chemical stability and are resistant to strong acid and alkali corrosion. They were first used in lead-acid batteries and can greatly increase the positive electrode oxygen evolution overpotential. Titanium oxide conductive ceramics have very unique physical, chemical and electrochemical properties. They are used in zinc-nickel batteries to solve the problems existing in the use of traditional zinc-nickel batteries and have good application prospects.
[0005] At present, titania conductive ceramics are required to have certain mechanical strength, excellent conductivity and corrosion resistance. Existing titania conductive ceramic materials are difficult to balance electrochemical properties and mechanical strength. Now there is a need to prepare a titania conductive ceramic material with high mechanical strength, excellent conductivity and corrosion resistance. Summary of the invention
[0006] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a titanium oxide ceramic with high mechanical strength and a preparation method thereof.
[0007] A titanium oxide ceramic with high mechanical strength, the raw materials of which include: anatase titanium oxide powder, butyl titanate, silane coupling agent, polyvinyl alcohol microspheres, N,N'-methylenebisacrylamide, diethylenetriamine, and additives; the mass ratio of anatase titanium oxide powder, butyl titanate, silane coupling agent, polyvinyl alcohol microspheres, N,N'-methylenebisacrylamide, diethylenetriamine, and additives is 10-30:20-40:1-2:5-15:2-4:1-3:1-2.
[0008] Preferably, the anatase titanium oxide powder is a submicron powder.
[0009] Preferably, the model of the silane coupling agent is KH550.
[0010] Preferably, the particle size of the polyvinyl alcohol microspheres is 1-100 μm.
[0011] Preferably, the auxiliary agent is at least one of carboxymethyl cellulose, polyethylene, polypropylene, polyvinyl butyral, polymethyl methacrylate, and polyimide, preferably carboxymethyl cellulose.
[0012] The method for preparing the above-mentioned titanium oxide ceramic with high mechanical strength comprises the following steps:
[0013] S1. Add polyvinyl alcohol microspheres to ethanol aqueous solution and disperse them evenly. Add butyl titanate thereto under nitrogen protection, stir for 10-30 minutes, keep warm at 70-80° C. for 20-40 minutes, filter, wash 2-3 times, dry, calcine at 400-500° C. for 10-20 hours under nitrogen protection, cool to room temperature, and crush to obtain activated titanium dioxide;
[0014] S2, adding activated titanium dioxide and silane coupling agent to ethanol aqueous solution, refluxing and stirring at 70-80°C for 2-4h, filtering, washing, drying, and then adding to methanol aqueous solution for ultrasonic treatment, adding N,N'-methylenebisacrylamide thereto, refluxing and stirring at 60-70°C for 10-15h, then adding diethylenetriamine, continuing to reflux and stir for 10-20h, washing, and vacuum drying to obtain grafted titanium dioxide;
[0015] S3. Evenly mix the grafted titanium dioxide, anatase titanium oxide powder and additives, ball-mill for 5-10 hours, press into shape, dry, heat to 1000-1200°C under nitrogen protection, calcine for 5-10 hours, maintain a vacuum degree of 8-10 kPa during the calcination process, naturally cool to room temperature, and stop nitrogen protection to obtain sub-titanium oxide ceramics with high mechanical strength.
[0016] Preferably, in S1, the mass fraction of the ethanol aqueous solution is 40-60%.
[0017] Preferably, in S2, the mass fraction of the ethanol aqueous solution is 40-60%, and the mass fraction of the methanol aqueous solution is 40-60%.
[0018] Preferably, in S2, the ultrasonic treatment frequency is 5-12 kHz, and the ultrasonic treatment time is 10-20 min.
[0019] Preferably, in S3, the pressing pressure is 5-15 MPa.
[0020] Preferably, in S3, the drying temperature is 90-110°C.
[0021] Preferably, in S3, the temperature is raised from room temperature to 1000-1200°C at a rate of 5-15°C / min under nitrogen protection.
[0022] The technical effects of the present invention are as follows:
[0023] The present invention adds butyl titanate to the ethanol water dispersion of polyvinyl alcohol microspheres. Since the surface of the polyvinyl alcohol microspheres contains a large number of hydroxyl groups, nano titanium dioxide is adsorbed on the surface of the polyvinyl alcohol microspheres through electrostatic action and precipitated. After high-temperature calcination, the polyvinyl alcohol microspheres are decomposed and carbonized to become a nano titanium dioxide carbon skeleton, which can not only effectively avoid the agglomeration of nano titanium dioxide, but also make it easier to expose more adsorption sites.
[0024] There are many hydroxyl groups on the surface of activated titanium dioxide, and the triethoxy group in the silane coupling agent KH550 reacts with the hydroxyl group to coat the surface of the activated titanium dioxide with organic groups, which not only enhances its reactivity with N,N'-methylenebisacrylamide and diethylenetriamine, but also the oxygen-containing functional groups on its surface can enhance the bonding strength; the activated titanium dioxide reacts with N,N'-methylenebisacrylamide and diethylenetriamine, and hyperbranched grafting is performed on the surface of the obtained activated titanium dioxide, which is then compounded with anatase-type titanium oxide powder and ball-milled, so that it can be fully dispersed into a highly branched structure.
[0025] The auxiliary agent can not only fully bond the grafted titanium dioxide and anatase titanium oxide powders, but also when the auxiliary agent is preferably carboxymethyl cellulose, its structural surface contains carboxyl groups, and the hyperbranched structure ends of the grafted titanium dioxide contain active amino groups. In the high temperature and high pressure process, the grafted titanium dioxide and carboxymethyl cellulose are cross-linked to promote the system to form a continuous network structure, thereby forming a matrix with a certain strength, and the anatase titanium oxide powder contacts and interweaves with each other in the hyperbranched polymer to form a conductive network with higher stability; after high-temperature calcination, the grafted titanium dioxide and the auxiliary agent are carbonized to form a three-dimensional inorganic macroporous carbon structure with sub-titanium oxide as the center and dispersed externally, and the sub-titanium oxide calcined product of the anatase titanium oxide powder is fully combined in the macroporous structure.
[0026] The present invention synthesizes Magnéli phase titanium oxide powder with large pores and hard structure, which has good conductivity, strong stability and good biocompatibility. Its highly dispersed pores are composed of an interwoven carbon skeleton with a thickness of up to 200nm. In addition, the electrode contains a large number of holes, which can provide more active sites for electrochemical reactions, thereby generating a large number of hydroxyl free radicals.
[0027] The titanium suboxide conductive ceramic electrode obtained by the present invention has good chemical reaction activity, wherein the diffusion path of oxygen is short, so the reaction time is short, which is beneficial to improving production efficiency and greatly shortening the production cycle of the titanium suboxide conductive ceramic electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the nitrogen isothermal adsorption-desorption curve of the titania ceramic obtained in Example 5.
[0029] Figure 2 The cyclic voltammetry curves of the zinc negative electrode prepared using the titania ceramics obtained in Example 5 and Comparative Examples 1-2.
[0030] Figure 3 The Tafel curves of the zinc negative electrode prepared using the titania ceramics obtained in Example 5 and Comparative Examples 1-2.
[0031] Figure 4 The AC impedance spectrum curves of the zinc negative electrode prepared using the sub-titanium oxide ceramics obtained in Example 5 and Comparative Examples 1-2. DETAILED DESCRIPTION
[0032] The present invention will be further explained below in conjunction with specific embodiments.
[0033] Example 1
[0034] A titanium oxide ceramic with high mechanical strength, the raw materials of which include: 10kg of submicron anatase titanium oxide powder, 20kg of butyl titanate, 1kg of silane coupling agent KH550, 5kg of polyvinyl alcohol microspheres with a particle size of 1-100μm, 2kg of N,N'-methylenebisacrylamide, 1kg of diethylenetriamine and 1kg of polyvinyl butyral.
[0035] The method for preparing the above-mentioned titanium oxide ceramic with high mechanical strength comprises the following steps:
[0036] S1. Add polyvinyl alcohol microspheres to 50 kg of 40% ethanol aqueous solution and disperse them evenly. Add butyl titanate thereto under nitrogen protection, stir at a speed of 1000 r / min for 10 min, keep warm at 70°C for 20 min, filter, wash twice with water and anhydrous ethanol alternately, dry, calcine at 400°C for 10 h under nitrogen protection, cool to room temperature, and crush to obtain activated titanium dioxide;
[0037] S2, adding activated titanium dioxide and silane coupling agent KH550 to 50kg of 40% ethanol aqueous solution, refluxing and stirring at 70°C for 2h, filtering, washing, drying, and then adding to 50kg of 40% methanol aqueous solution, ultrasonically treating at a frequency of 5kHz for 10min, adding N,N'-methylenebisacrylamide thereto, refluxing and stirring at 60°C for 10h, stirring at a speed of 50r / min, then adding diethylenetriamine, continuing to reflux and stir for 10h, washing, and vacuum drying to obtain grafted titanium dioxide;
[0038] S3. Evenly mix the grafted titanium dioxide, rutile titanium oxide powder and polyvinyl butyral, place them in a planetary ball mill and ball mill for 5 hours, add them to the mold, and then use a hydraulic press to press them. The pressing pressure is 5 MPa. After drying at 90°C, send them into a tubular furnace. Under nitrogen protection, heat from room temperature to 1000°C at a rate of 5°C / min, and calcine for 5 hours. Maintain the vacuum degree of 8 kPa during the calcination process, cool them naturally to room temperature, and stop nitrogen protection to obtain sub-titanium oxide ceramics with high mechanical strength.
[0039] Example 2
[0040] A titanium oxide ceramic with high mechanical strength, the raw materials of which include: 30kg of submicron anatase titanium oxide powder, 40kg of butyl titanate, 2kg of silane coupling agent KH550, 15kg of polyvinyl alcohol microspheres with a particle size of 1-100μm, 4kg of N,N'-methylenebisacrylamide, 3kg of diethylenetriamine, and 2kg of polyimide.
[0041] The method for preparing the above-mentioned titanium oxide ceramic with high mechanical strength comprises the following steps:
[0042] S1. Add polyvinyl alcohol microspheres to 100 kg of 60% ethanol aqueous solution and disperse them evenly. Add butyl titanate thereto under nitrogen protection, stir at a speed of 2000 r / min for 30 min, keep warm at 80°C for 40 min, filter, wash with water and anhydrous ethanol alternately for 3 times, dry, calcine at 500°C for 20 h under nitrogen protection, cool to room temperature, and crush to obtain activated titanium dioxide;
[0043] S2, adding activated titanium dioxide and silane coupling agent KH550 to 100 kg of 60% ethanol aqueous solution, refluxing and stirring at 80°C for 4 hours, filtering, washing, drying, and then adding to 100 kg of 60% methanol aqueous solution, ultrasonically treating at a frequency of 12 kHz for 20 minutes, adding N, N'-methylenebisacrylamide thereto, refluxing and stirring at 70°C for 15 hours, stirring at a speed of 150 r / min, then adding diethylenetriamine, continuing to reflux and stir for 20 hours, washing, and vacuum drying to obtain grafted titanium dioxide;
[0044] S3. Evenly mix the grafted titanium dioxide, rutile titanium oxide powder and polyimide, place them in a planetary ball mill and ball-mill for 10 hours, add them to the mold, and then use a hydraulic press to press them. The pressing pressure is 15MPa. After drying at 110°C, send them into a tubular furnace. Under nitrogen protection, heat from room temperature to 1200°C at a rate of 15°C / min, and calcine for 10 hours. During the calcination process, maintain the vacuum degree at 10kPa, cool naturally to room temperature, and stop nitrogen protection to obtain sub-titanium oxide ceramics with high mechanical strength.
[0045] Example 3
[0046] A titanium oxide ceramic with high mechanical strength, the raw materials of which include: 15kg of submicron anatase titanium oxide powder, 35kg of butyl titanate, 1.3kg of silane coupling agent KH550, 12kg of polyvinyl alcohol microspheres with a particle size of 1-100μm, 2.5kg of N,N'-methylenebisacrylamide, 2.5kg of diethylenetriamine, and 1.4kg of carboxymethyl cellulose.
[0047] The method for preparing the above-mentioned titanium oxide ceramic with high mechanical strength comprises the following steps:
[0048] S1. Add polyvinyl alcohol microspheres to 80 kg of 45% ethanol aqueous solution and disperse them evenly. Add butyl titanate thereto under nitrogen protection, stir at a speed of 1700 r / min for 15 min, keep warm at 77°C for 25 min, filter, wash with water and anhydrous ethanol alternately for 3 times, dry, calcine at 420°C for 18 h under nitrogen protection, cool to room temperature, and crush to obtain activated titanium dioxide;
[0049] S2, adding activated titanium dioxide and silane coupling agent KH550 to 70kg of 55% ethanol aqueous solution, refluxing and stirring at 73°C for 3.5h, filtering, washing, drying, and then adding to 60kg of 55% methanol aqueous solution, ultrasonically treating at a frequency of 6kHz for 17min, adding N,N'-methylenebisacrylamide, refluxing and stirring at 62°C for 14h, stirring at a speed of 80r / min, then adding diethylenetriamine, continuing to reflux and stir for 18h, washing, and vacuum drying to obtain grafted titanium dioxide;
[0050] S3. Evenly mix the grafted titanium dioxide, rutile titanium oxide powder and carboxymethyl cellulose, place them in a planetary ball mill for 6 hours, add them to the mold, and then use a hydraulic press to press them. The pressing pressure is 12MPa. After drying at 95°C, send them into a tubular furnace. Under nitrogen protection, heat from room temperature to 1050°C at a rate of 12°C / min, and calcine for 8 hours. During the calcination process, maintain the vacuum degree at 8.5kPa, cool them naturally to room temperature, and stop nitrogen protection to obtain sub-titanium oxide ceramics with high mechanical strength.
[0051] Example 4
[0052] A titanium oxide ceramic with high mechanical strength, the raw materials of which include: 25kg of submicron anatase titanium oxide powder, 25kg of butyl titanate, 1.7kg of silane coupling agent KH550, 8kg of polyvinyl alcohol microspheres with a particle size of 1-100μm, 3.5kg of N,N'-methylenebisacrylamide, 1.5kg of diethylenetriamine, and 1.8kg of carboxymethyl cellulose.
[0053] The method for preparing the above-mentioned titanium oxide ceramic with high mechanical strength comprises the following steps:
[0054] S1. Add polyvinyl alcohol microspheres to 60 kg of 55% ethanol aqueous solution and disperse them evenly. Add butyl titanate thereto under nitrogen protection, stir at a speed of 1300 r / min for 25 min, keep warm at 73°C for 35 min, filter, wash twice with water and anhydrous ethanol alternately, dry, calcine at 480°C for 12 h under nitrogen protection, cool to room temperature, and crush to obtain activated titanium dioxide;
[0055] S2, adding activated titanium dioxide and silane coupling agent KH550 to 90kg of 45% ethanol aqueous solution, refluxing and stirring at 77°C for 2.5h, filtering, washing, drying, and then adding to 80kg of 45% methanol aqueous solution, ultrasonically treating at a frequency of 10kHz for 13min, adding N,N'-methylenebisacrylamide, refluxing and stirring at 68°C for 12h, stirring at a speed of 120r / min, then adding diethylenetriamine, continuing to reflux and stir for 12h, washing, and vacuum drying to obtain grafted titanium dioxide;
[0056] S3. Evenly mix the grafted titanium dioxide, rutile titanium oxide powder and carboxymethyl cellulose, place them in a planetary ball mill for 8 hours, add them to the mold, and then use a hydraulic press to press them. The pressing pressure is 8 MPa. After drying at 105°C, send them to a tubular furnace. Under nitrogen protection, heat from room temperature to 1150°C at a rate of 8°C / min, and calcine for 6 hours. During the calcination process, maintain the vacuum degree at 9.5 kPa, cool them naturally to room temperature, and stop nitrogen protection to obtain sub-titanium oxide ceramics with high mechanical strength.
[0057] Example 5
[0058] A titanium oxide ceramic with high mechanical strength, the raw materials of which include: 20kg of submicron anatase titanium oxide powder, 30kg of butyl titanate, 1.5kg of silane coupling agent KH550, 10kg of polyvinyl alcohol microspheres with a particle size of 1-100μm, 3kg of N,N'-methylenebisacrylamide, 2kg of diethylenetriamine, and 1.6kg of carboxymethyl cellulose.
[0059] The method for preparing the above-mentioned titanium oxide ceramic with high mechanical strength comprises the following steps:
[0060] S1. Add polyvinyl alcohol microspheres to 70 kg of 50% ethanol aqueous solution and disperse them evenly. Add butyl titanate under nitrogen protection, stir at a speed of 1500 r / min for 20 min, keep warm at 75°C for 30 min, filter, wash with water and anhydrous ethanol alternately for 3 times, dry, calcine at 450°C for 15 h under nitrogen protection, cool to room temperature, and crush to obtain activated titanium dioxide;
[0061] S2, adding activated titanium dioxide and silane coupling agent KH550 to 80 kg of 50% ethanol aqueous solution, refluxing and stirring at 75°C for 3 hours, filtering, washing, drying, and then adding to 70 kg of 50% methanol aqueous solution, ultrasonically treating at a frequency of 8 kHz for 15 minutes, adding N, N'-methylenebisacrylamide, refluxing and stirring at 65°C for 13 hours, stirring at a speed of 100 r / min, then adding diethylenetriamine, continuing to reflux and stir for 15 hours, washing, and vacuum drying to obtain grafted titanium dioxide;
[0062] S3. Evenly mix the grafted titanium dioxide, rutile titanium oxide powder and carboxymethyl cellulose, place them in a planetary ball mill for 7 hours, add them to the mold, and then use a hydraulic press to press them. The pressing pressure is 10MPa. After drying at 100°C, send them into a tubular furnace. Under nitrogen protection, heat from room temperature to 1100°C at a rate of 10°C / min, and calcine for 7 hours. During the calcination process, maintain the vacuum degree at 9kPa, naturally cool to room temperature, and stop nitrogen protection to obtain sub-titanium oxide ceramics with high mechanical strength.
[0063] The Vickers hardness of the titania ceramic obtained in this embodiment was tested, and its hardness could reach 367 HV, which is better than the commercially available titania ceramic electrode material (230 HV), confirming that the titania ceramic obtained in this application has high mechanical strength.
[0064] The BET nitrogen isothermal adsorption method was used to characterize the titanium oxide ceramics obtained in this example. Figure 1 As shown, it can be seen that the nitrogen adsorption amount in the low-pressure section increases slowly, while the adsorption amount in the high-pressure section increases rapidly. The applicant believes that this is because the main body of the titania ceramic is a three-dimensional inorganic macroporous carbon structure with titania as the center and dispersed externally, and the calcined product of rutile titanium oxide powder is titanium oxide that is fully combined in the macroporous structure.
[0065] Comparative Example 1
[0066] A titanium oxide ceramic with high mechanical strength, the raw materials of which include: 20kg of submicron anatase titanium oxide powder, 30kg of butyl titanate, 1.5kg of silane coupling agent KH550, 3kg of N,N'-methylenebisacrylamide, 2kg of diethylenetriamine, and 1.6kg of carboxymethyl cellulose.
[0067] The method for preparing the above-mentioned titanium oxide ceramic with high mechanical strength comprises the following steps:
[0068] i. Add butyl titanate and silane coupling agent KH550 to 80 kg of 50% ethanol aqueous solution, reflux and stir at 75°C for 3 hours, filter, wash, dry, then add to 70 kg of 50% methanol aqueous solution, ultrasonically treat at a frequency of 8 kHz for 15 minutes, add N,N'-methylenebisacrylamide, reflux and stir at 65°C for 13 hours at a stirring speed of 100 r / min, then add diethylenetriamine, continue reflux and stir for 15 hours, wash, and vacuum dry to obtain grafted titanium dioxide;
[0069] ii. Mix the grafted titanium dioxide, anatase titanium oxide powder and carboxymethyl cellulose evenly, place them in a planetary ball mill for 7 hours, add them to a mold, and then use a hydraulic press to press them. The pressing pressure is 10MPa. After drying at 100°C, send them into a tubular furnace. Under nitrogen protection, heat from room temperature to 1100°C at a rate of 10°C / min, and calcine for 7 hours. Maintain a vacuum degree of 9kPa during the calcination process, cool them naturally to room temperature, and stop nitrogen protection to obtain sub-titanium oxide ceramics with high mechanical strength.
[0070] Comparative Example 2
[0071] A titanium oxide ceramic with high mechanical strength, the raw materials of which include: 20kg of submicron anatase titanium oxide powder, 30kg of butyl titanate, 10kg of polyvinyl alcohol microspheres with a particle size of 1-100μm, and 1.6kg of carboxymethyl cellulose.
[0072] The method for preparing the above-mentioned titanium oxide ceramic with high mechanical strength comprises the following steps:
[0073] i. Add polyvinyl alcohol microspheres to 70 kg of 50% ethanol aqueous solution and disperse them evenly. Add butyl titanate thereto under nitrogen protection, stir at a speed of 1500 r / min for 20 min, keep warm at 75°C for 30 min, filter, wash with water and anhydrous ethanol alternately for 3 times, dry, calcine at 450°C for 15 h under nitrogen protection, cool to room temperature, and crush to obtain activated titanium dioxide;
[0074] ii. Mix activated titanium dioxide, rutile titanium oxide powder and carboxymethyl cellulose evenly, place them in a planetary ball mill for 7 hours, add them to a mold, and then use a hydraulic press to press them. The pressing pressure is 10MPa. After drying at 100°C, send them into a tubular furnace. Under nitrogen protection, heat from room temperature to 1100°C at a rate of 10°C / min, and calcine for 7 hours. During the calcination process, maintain a vacuum degree of 9kPa, cool them naturally to room temperature, and stop nitrogen protection to obtain sub-titanium oxide ceramics with high mechanical strength.
[0075] The titanium oxide ceramics obtained in Example 5 and Comparative Examples 1-2 were used to prepare zinc negative electrodes by a slurry coating method. First, the active material zinc oxide of the zinc negative electrode, the binder tetrafluoroethylene, sodium hydroxymethyl cellulose and each group of titanium oxide ceramics were weighed in a mass ratio of 90:4:3:3, placed in a mortar and ground evenly, deionized water was added and stirred continuously to form a viscous slurry, the slurry was evenly coated on the brass mesh current collector, and then dried at room temperature and pressed into sheets, and cut into 2 cm×2 cm zinc negative electrodes.
[0076] The electrochemical performance test of the zinc negative electrode was carried out using a three-electrode system, with the zinc negative electrode as the working electrode, the sintered nickel electrode as the auxiliary electrode, the Hg / HgO electrode as the reference electrode, and the electrolyte being a 6 mol / L potassium hydroxide solution saturated with zinc oxide. The electrochemical performance test includes: cyclic voltammetry curve, Tafel curve and AC impedance spectrum.
[0077] a. Cyclic voltammetry curve test was carried out on RST-5000 electrochemical workstation with a scan speed of 20 mV / s.
[0078] like Figure 2 As shown, the current peaks of the three are between -1.0 and -1.6 V, among which the potential difference of the redox peak of the Example 5 group is the smallest, which means that the zinc negative electrode prepared by the sub-titania ceramic obtained in Example 5 has better reversibility. The voltage corresponding to the current peak of the Example 5 group is smaller, indicating that the discharge reaction can be carried out at a lower voltage, and the zinc negative electrode has better discharge performance.
[0079] b. Tafel curve test was performed on RST-5000 electrochemical workstation with a scan speed of 0.1 mV / s.
[0080] like Figure 3 As shown, the corrosion potential of Example 5 is higher. After conversion, it can be concluded that the corrosion inhibition efficiency of Example 5 is also the highest, indicating that the zinc negative electrode of Example 5 has better corrosion resistance. The applicant believes that this is because the present application uses activated titanium dioxide to react with N, N'-methylenebisacrylamide and diethylenetriamine, and hyperbranched grafting is performed on the surface of the activated titanium dioxide obtained, and then ball milled with anatase titanium oxide powder, which can be fully dispersed into a highly branched structure; and in the high temperature and high pressure process, the grafted titanium dioxide and carboxymethyl cellulose cross-link to promote the system to form a continuous network structure, thereby forming a matrix with a certain strength, and the anatase titanium oxide powder contacts and interweaves with each other in the hyperbranched polymer to form a conductive network. Then the obtained sub-titania ceramic is used to prepare the zinc negative electrode. On the one hand, the obtained sub-titania ceramic has excellent corrosion resistance, and on the other hand, zinc oxide is uniformly deposited on the surface of the zinc negative electrode, so that the current is evenly distributed, effectively inhibiting the growth of dendrites, and keeping the zinc negative electrode in its inherent shape during the charge and discharge process, thereby further improving the corrosion resistance.
[0081] c. The AC impedance spectrum test was carried out on a CHI660G electrochemical workstation with an AC signal amplitude of 5 mV and a frequency range of 0.01-100 kHz.
[0082] like Figure 4 As shown, the trends of the zinc negative electrodes of each group are similar, and are composed of a semicircle in the high-frequency region and a straight line in the low-frequency region. By fitting the curve in the figure, it is found that the charge transfer resistance of the zinc negative electrode of Example 5 is the smallest, indicating that the conductivity of the zinc negative electrode of Example 5 is the best, which confirms that the sub-titanium oxide ceramic obtained in Example 5 has excellent conductivity.
[0083] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A titanium oxide ceramic with high mechanical strength, characterized in that: The raw materials include: anatase titanium oxide powder, butyl titanate, silane coupling agent, polyvinyl alcohol microspheres, N,N'-methylenebisacrylamide, diethylenetriamine, and additives; the mass ratio of anatase titanium oxide powder, butyl titanate, silane coupling agent, polyvinyl alcohol microspheres, N,N'-methylenebisacrylamide, diethylenetriamine, and additives is 10-30:20-40:1-2:5-15:2-4:1-3:1-2; Prepared by the following steps: S1. Add polyvinyl alcohol microspheres to ethanol aqueous solution and disperse them evenly. Add butyl titanate thereto under nitrogen protection, stir for 10-30 minutes, keep warm at 70-80° C. for 20-40 minutes, filter, wash 2-3 times, dry, calcine at 400-500° C. for 10-20 hours under nitrogen protection, cool to room temperature, and crush to obtain activated titanium dioxide; S2, adding activated titanium dioxide and silane coupling agent to ethanol aqueous solution, refluxing and stirring at 70-80°C for 2-4h, filtering, washing, drying, and then adding to methanol aqueous solution for ultrasonic treatment, adding N,N'-methylenebisacrylamide thereto, refluxing and stirring at 60-70°C for 10-15h, then adding diethylenetriamine, continuing to reflux and stir for 10-20h, washing, and vacuum drying to obtain grafted titanium dioxide; S3. Evenly mix the grafted titanium dioxide, anatase titanium oxide powder and additives, ball-mill for 5-10 hours, press into shape, dry, heat to 1000-1200°C under nitrogen protection, calcine for 5-10 hours, maintain a vacuum degree of 8-10 kPa during the calcination process, naturally cool to room temperature, and stop nitrogen protection to obtain sub-titanium oxide ceramics with high mechanical strength.
2. The titanium oxide ceramic with high mechanical strength according to claim 1, characterized in that: Anatase titanium oxide powder is a submicron powder.
3. The titanium oxide ceramic with high mechanical strength according to claim 1, characterized in that: The model of the silane coupling agent is KH550.
4. The titanium oxide ceramic with high mechanical strength according to claim 1, characterized in that: The particle size of the polyvinyl alcohol microspheres is 1-100 μm.
5. The titanium oxide ceramic with high mechanical strength according to claim 1, characterized in that: The auxiliary agent is at least one of carboxymethyl cellulose, polyethylene, polypropylene, polyvinyl butyral, polymethyl methacrylate and polyimide.
6. A method for preparing a titanium oxide ceramic with high mechanical strength as claimed in any one of claims 1 to 5, characterized in that: The steps include: S1. Add polyvinyl alcohol microspheres to ethanol aqueous solution and disperse them evenly. Add butyl titanate thereto under nitrogen protection, stir for 10-30 minutes, keep warm at 70-80° C. for 20-40 minutes, filter, wash 2-3 times, dry, calcine at 400-500° C. for 10-20 hours under nitrogen protection, cool to room temperature, and crush to obtain activated titanium dioxide; S2, adding activated titanium dioxide and silane coupling agent to ethanol aqueous solution, refluxing and stirring at 70-80°C for 2-4h, filtering, washing, drying, and then adding to methanol aqueous solution for ultrasonic treatment, adding N,N'-methylenebisacrylamide thereto, refluxing and stirring at 60-70°C for 10-15h, then adding diethylenetriamine, continuing to reflux and stir for 10-20h, washing, and vacuum drying to obtain grafted titanium dioxide; S3. Evenly mix the grafted titanium dioxide, anatase titanium oxide powder and additives, ball-mill for 5-10 hours, press into shape, dry, heat to 1000-1200°C under nitrogen protection, calcine for 5-10 hours, maintain a vacuum degree of 8-10 kPa during the calcination process, naturally cool to room temperature, and stop nitrogen protection to obtain sub-titanium oxide ceramics with high mechanical strength.
7. The method for preparing titanium oxide ceramics with high mechanical strength according to claim 6, characterized in that: In S1, the mass fraction of the ethanol aqueous solution is 40-60%.
8. The method for preparing titanium oxide ceramics with high mechanical strength according to claim 6, characterized in that: In S2, the mass fraction of the ethanol aqueous solution is 40-60%, and the mass fraction of the methanol aqueous solution is 40-60%.
9. The method for preparing titanium oxide ceramics with high mechanical strength according to claim 6, characterized in that: In S2, the ultrasonic treatment frequency is 5-12 kHz, and the ultrasonic treatment time is 10-20 min.
10. The method for preparing titanium oxide ceramics with high mechanical strength according to claim 6, characterized in that: In S3, the pressing pressure is 5-15 MPa.