A high entropy perovskite ceramic material with submicron fine crystal structure and preparation method thereof

By preparing high-entropy perovskite ceramic materials with sub-micron fine-grained structures, the problems of insufficient energy density and efficiency of existing high-entropy ceramic materials are solved, and electrical properties of high breakdown field strength and high efficiency are achieved, which is suitable for electronic components. miniaturization needs.

CN116986902BActive Publication Date: 2024-10-15SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311054536.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-21
Publication Date
2024-10-15
Estimated Expiration
2043-08-21

AI Technical Summary

Technical Problem

The recyclable energy density and efficiency of existing high-entropy ceramic materials cannot meet market demand, and ceramic materials with the simultaneous presence of five elements and their preparation methods are relatively scarce.

Method used

High-entropy perovskite ceramic material with submicron fine-grained structure (chemical composition is (Na1/8Ba1/4Ca1/4Sr1/4Bi1/8)(Y1/8Zr1/4Sn1/4Ti1/4Nb1 /8)O3), prepared through specific mixing, ball milling, drying, briquetting, pre-calcination, granulation and sintering steps, combined with solid-phase method and high-temperature sintering technology, optimizing the doping amount of Na2CO3 and Bi2O3 to improve material performance .

Benefits of technology

It achieves the submicron microstructure of ceramic materials, improves the breakdown field strength and recyclable energy density, and obtains high-efficiency electrical properties, which is suitable for large-scale applications and miniaturization development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116986902B_ABST
    Figure CN116986902B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-entropy perovskite ceramic material with a submicron fine-grained structure and a preparation method. On the basis of ABO3, the A position and the B position are respectively doped with a solid solution synthesized by five elements, and then the high-entropy perovskite ceramic material is prepared by combining a solid phase method and a specific preparation process. The obtained high-entropy perovskite ceramic material has a submicron microstructure with an extremely small grain size, which is conducive to the improvement of the breakdown field strength in the ceramic, and it is easier to obtain a large recoverable energy density and efficiency. The present invention applies the concept of high entropy to dielectric ceramic materials. Considering the volatilization of Na2CO3 and Bi2O3 during the sintering process, the materials are over-doped, and the influence of different doping contents on the phase structure of high-entropy perovskite ceramic materials is explored and the optimal doping is obtained, so that the experimental results are more convincing. By combining multiple principal elements and utilizing the unique effects of high-entropy materials, the performance is improved, providing new ideas for the design of dielectric ceramic materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of dielectric ceramic materials and relates to a high-entropy perovskite ceramic material with a submicron fine-grained structure and a preparation method thereof. Background Art

[0002] With the continuous development of science and technology, the demand for miniaturization of electronic components is increasing. Dielectric capacitors have the advantages of high power density, fast charging and discharging, and long cycle life. They are an important component of microelectronic devices and are irreplaceable in the field of electronics. However, the main research bottleneck is the relatively low recoverable energy density and the risk of thermal loss breakdown, which hinders the large-scale application of dielectric energy storage devices and their development towards miniaturization.

[0003] As people's demand for new materials becomes increasingly urgent, the development of new dielectric ceramics with excellent performance has become a research hotspot for scientists. In recent years, the unconventional material design concept of "high entropy" has been proposed and has become a new strategy in the field of dielectric energy storage research. Due to its excellent performance, the concept of high entropy has attracted widespread attention from researchers and extended to the fields of high entropy ceramics and composite materials, providing new opportunities for the composition design and performance regulation of new materials. High entropy ceramics are a type of single-phase ceramic material with a multi-principal component composition. From the perspective of chemical composition, high entropy ceramics are considered to be a solid solution formed by the presence of five or more elements at a single site in a similar or equal molar ratio between the elements. From the perspective of entropy, high entropy ceramics are multi-principal component solid solutions with a configuration entropy greater than 1.5R (R is the gas constant), which are characterized by long-range order in the crystal structure and long-range disorder in the chemical composition. The special effects brought about by its multi-principal component composition and the broad exploration space make it a hot topic in the field of ceramics. The design concept of high-entropy ceramics is completely different from that of traditional ceramics. Compared with traditional ceramic materials with a single main element, high-entropy ceramics select five or more metal elements as the main elements at the same time. The atomic ratio of the metal elements is equal or nearly equal, and its composition is located in the center of the ternary or quaternary phase diagram. The composition design is huge. Due to the high configurational entropy, the Gibbs free energy of the system is reduced, the structural stability is increased, and a uniform and single high-entropy phase can be formed even when containing multiple elements. Due to the disorder of its internal structure, four major effects are produced in the high-entropy system with highly disordered elements, including the thermodynamic high-entropy effect, the hysteresis diffusion effect in kinetics, the structural lattice distortion effect, and the synergistic effect of the components.

[0004] In 2004, Professor Ye Junwei first proposed the concept of high entropy alloys, which attracted widespread attention due to their high hardness, high stability and high wear resistance. In 2015, Rost et al. first reported a rock salt structure entropy-stabilized oxide ceramic, and the concept of high entropy oxide was proposed. Subsequently, more and more high entropy ceramics gradually became research progress. Yang et al. successfully prepared single-phase perovskite structure high entropy ceramics (Bi 0.2 Na 0.2 K 0.2 La 0.2 Sr 0.2 )TiO 3 , showing a dense nanostructure with fine grain size, improving the breakdown field strength in ceramics. Chen et al. successfully synthesized high entropy ceramics (Na 0.2 Bi 0.2 Ca 0.2 Sr 0.2 Ba 0.2 )TiO 3 , showing relaxation behavior, can obtain large recyclable energy density and high efficiency. However, although the electrical properties of the material have been improved by introducing the concept of high entropy, the recyclable energy density and efficiency still cannot meet the market demand, and there is still a lot of room for exploration. At present, there are few reports on ceramic materials with 5 elements at the A and B positions and their preparation methods. Summary of the invention

[0005] The purpose of the present invention is to solve the problem that the recyclable energy density and efficiency of ceramic materials prepared by high entropy in the prior art cannot meet market demand, and to provide a high entropy perovskite ceramic material with a submicron fine-grained structure and a preparation method.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention proposes a high entropy perovskite ceramic material with a submicron fine crystal structure, and the chemical composition of the high entropy perovskite ceramic material is (Na 1 / 8 Ba 1 / 4 Ca 1 / 4 Sr 1 / 4 Bi 1 / 8 )(Y 1 / 8 Zr 1 / 4 Sn 1 / 4 Ti 1 / 4 Nb 1 / 8 ) 3 , with a microscopic grain structure.

[0008] The present invention provides a method for preparing a high-entropy perovskite ceramic material with a submicron fine-grained structure, comprising the following steps:

[0009] Step 1: Na2 CO 3 、SrCO 3 、TiO 2 、BaCO 3 SnO 2 , Nb 2 O 5 、CaCO 3 、Bi 2 O 3 , Y 2 O 3 and ZrO 2 Mixing to obtain mixture A;

[0010] Step 2: ball milling, drying and briquetting the mixture A in sequence, and then pre-sintering to form a main crystal phase powder;

[0011] Step 3, the pre-sintered main crystal phase powder is subjected to ball milling, drying, granulation and sieving in sequence to obtain powder particles;

[0012] Step 4: Press the powder particles into a ceramic green body, sinter until cooled to room temperature, and obtain a high entropy perovskite ceramic material.

[0013] Preferably, in step 1, Na 2 CO 3 、SrCO 3 、TiO 2 、BaCO 3 SnO 2 , Nb 2 O 5 、CaCO 3 、Bi 2 O 3 , Y 2 O 3 and ZrO 2 The molar ratio is 1:4:4:4:4:1:4:1:1:4.

[0014] Preferably, in step 2, the ball milling time is 12 hours; the drying time is 1 hour to 2 hours, and the drying temperature is 100°C to 120°C; the pre-firing time is 3 hours to 4 hours, and the pre-firing temperature is 1200°C to 1240°C.

[0015] Preferably, in step 2, zirconium spheroidite and anhydrous ethanol are added to mixture A during ball milling, and mixture A, zirconium spheroidite and anhydrous ethanol are mixed in a mass ratio of 1:2:1.

[0016] Preferably, in step three, the sintered powder is first ground into fine powder and passed through a 120-mesh sieve, and then ball milled.

[0017] Preferably, in step three, granulation and sieving are performed by slowly dropping an appropriate amount of a binder with a concentration of 4wt% to 6wt% with a dropper during the grinding process of the powder, and filtering with a 60-mesh sieve to obtain a uniform powder.

[0018] Preferably, in step three, the binder is a polyvinyl alcohol solution.

[0019] Preferably, in step 4, the granulated powder particles are pressed into a ceramic green body at a pressure of 8 MPa to 12 MPa.

[0020] Preferably, in step four, the ceramic green body is sintered, the temperature is increased from room temperature to 500°C to 600°C at a rate of 3°C / min to 5°C / min, and kept for 120min to 140min for debinding, the temperature is continued to be increased to 1400°C to 1450°C and kept for 3h to 4h, and then the temperature is decreased to 600°C to 700°C at a rate of 3°C / min to 5°C / min until it is cooled to room temperature to obtain a high entropy perovskite ceramic material.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The high entropy perovskite ceramic material with a submicron fine-grained structure proposed by the present invention has a submicron microstructure with extremely small grain size, and the grains are tightly bound, with almost no obvious gaps, and has good compactness. Small grain size is conducive to improving the breakdown field strength in the ceramic, making it easier to obtain large recyclable energy density and efficiency.

[0023] The present invention proposes a method for preparing a high entropy perovskite ceramic material with a submicron fine-grained structure. 3 On the basis of the invention, the A and B positions are doped with five elements to synthesize a solid solution, and then the solid phase method and a specific preparation process are combined to prepare a high entropy perovskite ceramic material. The obtained high entropy perovskite ceramic material has a submicron microstructure with a very small grain size, which is beneficial to the improvement of the breakdown field strength in the ceramic and makes it easier to obtain a large recoverable energy density and efficiency. The specific invention applies the concept of high entropy to dielectric ceramic materials. Considering the Na 2 CO 3 、Bi 2 O 3 The volatilization phenomenon is studied by over-doping it and exploring the influence of different doping contents on the phase structure of high-entropy perovskite ceramic materials. The experimental results are more convincing. Through the combination of multiple principal elements and the use of the unique effects of high-entropy materials, the high-entropy strategy breaks the conventional material design concept, improves its performance, and provides new ideas for the design of dielectric ceramic materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0025] Figure 1 This is a flow chart of the method for preparing a high-entropy perovskite ceramic material with a submicron fine-grained structure of the present invention.

[0026] Figure 2 This is the SEM image of Example 3 of the present invention.

[0027] Figure 3 This is a graph showing the average grain size of Example 3 of the present invention.

[0028] Figure 4 This is the SEM image of Example 6 of the present invention.

[0029] Figure 5 This is a graph showing the average grain size of Example 6 of the present invention.

[0030] Figure 6 This is the SEM image of Example 8 of the present invention.

[0031] Figure 7 This is a graph showing the average grain size of Example 8 of the present invention.

[0032] Figure 8 It is a single-sided PE curve diagram of Example 3 of the present invention under different electric fields.

[0033] Fig. 9 This is a graph showing how the energy storage density and efficiency vary with the electric field in Example 3 of the present invention. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0035] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0037] In the description of the embodiments of the present invention, it should be noted that if the terms "upper", "lower", "horizontal", "inner", etc. indicate an orientation or positional relationship based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship in which the product of the invention is usually placed when in use, it is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.

[0038] In addition, if the term "horizontal" appears, it does not mean that the component must be absolutely horizontal, but can be slightly tilted. For example, "horizontal" only means that its direction is more horizontal than "vertical", which does not mean that the structure must be completely horizontal, but can be slightly tilted.

[0039] In the description of the embodiments of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal connection of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0040] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0041] The present invention proposes a high entropy perovskite ceramic material with a submicron fine-grained structure, the components of which are (Na 1 / 8 Ba 1 / 4 Ca 1 / 4 Sr 1 / 4 Bi 1 / 8 )(Y 1 / 8 Zr 1 / 4 Sn 1 / 4 Ti 1 / 4 Nb 1 / 8 ) 3 It has a super fine microscopic grain structure with a grain size of 0.34um. 3 On the basis of this, five elements are doped at the A and B sites respectively to synthesize the solid solution.

[0042] In the preparation method of the present invention, Na 2 CO 3 、SrCO 3 、TiO 2 、BaCO 3 SnO 2 , Nb 2 O 5 、CaCO 3 、Bi 2 O 3 , Y 2 O 3 and ZrO 2 Mix and dope with appropriate amount of Na 2 CO 3 、Bi 2 O 3 The synthetic mixed powder is prepared by solid phase method, such as Figure 1 As shown, the following steps are included:

[0043] Step 1: Na 2 CO 3 、SrCO 3 、TiO 2 、BaCO 3 SnO 2 , Nb 2 O 5 、CaCO 3 、Bi 2 O 3 , Y 2 O 3 and ZrO 2 Mixing to obtain mixture A;

[0044] Step 2: ball milling, drying and briquetting the mixture A in sequence, and then pre-sintering to form a main crystal phase powder;

[0045] Step 3, the pre-sintered main crystal phase powder is subjected to ball milling, drying, granulation and sieving in sequence to obtain powder particles;

[0046] Step 4: Press the powder particles into a ceramic green body, sinter until cooled to room temperature, and obtain a high entropy perovskite ceramic material.

[0047] The specific steps include:

[0048] Step 1: Prepare the ingredients according to the reaction equation and the required quantity of the required drug, using Na 2 CO 3 、SrCO 3 、TiO 2 、BaCO 3 SnO 2 , Nb2 O 5 、CaCO 3 、Bi 2 O 3 , Y 2 O 3 and ZrO 2 As raw materials, weigh them in a molar ratio of 1:4:4:4:4:1:4:1:4, and dope them with 1% to 5% mol of Na 2 CO 3 、Bi 2 O 3 A mixture A is obtained;

[0049] Step 2: Mix mixture A, zirconium spherulite and anhydrous ethanol in a mass ratio of 1:2:1 and put them into a ball mill for 12 hours. Take out the wet slurry after ball milling and pour it into a petri dish for drying. The drying time is 1 to 2 hours and the drying temperature is 100 to 120°C. After briquetting, put it into a high-temperature furnace and pre-sinter it at a temperature of 1200 to 1240°C for 3 to 4 hours to form a main crystal phase powder for use;

[0050] Step 3: The sintered powder is first ground into fine powder and passed through a 120-mesh sieve, and the obtained finer powder is subjected to secondary ball milling. In the secondary ball milling, the pre-burned powder after the previous step is mixed with zirconium ball stone and anhydrous ethanol in a mass ratio of 1:2:1 and ball milled for 12 hours. After drying, a suitable 4-6wt% PVA adhesive is dripped into the powder with a dropper in small amounts and the adhesive is added. The grinding rod is continuously stirred to obtain particles of uniform size, and the powder is passed through a 60-mesh sieve to obtain powder particles for pressing ceramics;

[0051] Step 4: Press the powder particles into a ceramic green body at a pressure of 8-12 MPa, sinter the ceramic green body in a high-temperature furnace, heat it from room temperature to 500-600°C at 3-5°C / min, and keep it warm for 120-140min to debind, continue to heat it to 1400-1450°C and keep it warm for 3-4h, then cool it to 600-700°C at 3-5°C / min until it cools to room temperature, and obtain a high entropy perovskite ceramic pretreated sample;

[0052] Step 5: Polish and clean the ceramic sample sintered in step 4, evenly coat the front and back sides of the sample with silver electrode slurry, and heat it at 500-600° C. for 20-40 minutes to obtain a high entropy perovskite ceramic sample.

[0053] In order to enable those skilled in the art to understand the purpose, content and technical solution of the present invention more clearly, the invention can be realized according to the described content without further creative work. A plurality of specific implementation methods are selected and combined with the accompanying drawings to describe the technical solution of the present invention in a clearer, more detailed and understandable manner.

[0054] Embodiment 1:

[0055] Step 1: Prepare the ingredients according to the reaction equation and the required quantity of the required drug, using Na 2 CO 3 、SrCO 3 、TiO 2 、BaCO 3 SnO 2 , Nb 2 O 5 、CaCO 3 、Bi 2 O 3 , Y 2 O 3 and ZrO 2 As raw materials, the molar ratio is 1:4:4:4:4:1:4:1:4, and 1% mol of Na 2 CO 3 、1%mol Bi 2 O 3 A mixture A is obtained;

[0056] Step 2: The mixture A, zirconium spheroids and anhydrous ethanol are ball milled, dried and briquette-pressed in a mass ratio of 1:2:1, and then placed in a high-temperature furnace for pre-calcination at a temperature of 1210°C for 3 hours to form a main crystal phase powder for standby use;

[0057] Step 3: The pre-sintered powder is ball-milled, dried, granulated and sieved in sequence to obtain powder particles for pressing ceramics;

[0058] In step 3 and step 4, the ball milling time is 12 hours; the drying time is 2 hours, and the drying temperature is 120°C; the sintered powder is sieved through a 120-mesh sieve; granulation and sieving are performed by dropping an appropriate amount of 6wt% PVA adhesive into the powder, mixing it thoroughly, and sieving it through a 60-mesh sieve;

[0059] Step 4: Press the powder particles into a ceramic green body at a pressure of 12 MPa, sinter the ceramic green body in a high-temperature furnace, heat it from room temperature to 600 ° C at 5 ° C / min, and keep it at this temperature for 120 minutes to debind, continue to heat it to 1400 ° C and keep it at this temperature for 4 hours, and then cool it to 700 ° C at 3 ° C / min until it cools to room temperature;

[0060] Step 5: Polish, grind and clean the ceramic sample sintered in step 4, evenly coat the front and back sides of the sample with silver electrode slurry, and heat it at 600°C for 30 minutes to obtain a high entropy perovskite ceramic sample.

[0061] Embodiment 2:

[0062] Step 1: Prepare the ingredients according to the reaction equation and the required quantity of the required drug, using Na 2 CO 3 、SrCO 3 、TiO 2 、BaCO 3 SnO 2 , Nb 2 O 5 、CaCO 3 、Bi 2 O 3 , Y 2 O 3 and ZrO 2 As raw materials, the molar ratio is 1:4:4:4:4:1:4:1:4, and 2% mol of Na 2 CO 3 、1%mol Bi 2 O 3 A mixture A is obtained;

[0063] Step 2: The mixture A, zirconium spheroids and anhydrous ethanol are ball milled, dried and briquette-pressed in a mass ratio of 1:2:1, and then placed in a high-temperature furnace for pre-calcination at 1220°C for 3 hours to form a main crystal phase powder for standby use;

[0064] Step 3: The pre-sintered powder is ball-milled, dried, granulated and sieved in sequence to obtain powder particles for pressing ceramics;

[0065] In step 3 and step 4, the ball milling time is 12 hours; the drying time is 2 hours, and the drying temperature is 120°C; the sintered powder is sieved through a 120-mesh sieve; granulation and sieving are performed by dropping an appropriate amount of 6wt% PVA adhesive into the powder, mixing it thoroughly, and sieving it through a 60-mesh sieve;

[0066] Step 4: Press the powder particles into a ceramic green body under a pressure of 12 MPa, sinter the ceramic green body in a high-temperature furnace, heat it from room temperature to 600°C at a rate of 5°C / min, and keep it at that temperature for 140 minutes to debind, continue to heat it to 1410°C and keep it at that temperature for 4 hours, and then cool it down to 700°C at a rate of 3°C / min until it cools to room temperature;

[0067] Step 5: Polish, grind and clean the ceramic sample sintered in step 4, evenly coat the front and back sides of the sample with silver electrode slurry, and heat it at 600°C for 30 minutes to obtain a high entropy perovskite ceramic sample.

[0068] Embodiment 3:

[0069] Step 1: Prepare the ingredients according to the reaction equation and the required quantity of the required drug, using Na 2 CO 3 、SrCO3 、TiO 2 、BaCO 3 SnO 2 , Nb 2 O 5 、CaCO 3 、Bi 2 O 3 , Y 2 O 3 and ZrO 2 As raw materials, the molar ratio is 1:4:4:4:4:1:4:1:4, and 3% mol of Na 2 CO 3 、1%mol Bi 2 O 3 A mixture A is obtained;

[0070] Step 2: The mixture A, zirconium spheroids and anhydrous ethanol are ball milled, dried and briquette-pressed in a mass ratio of 1:2:1, and then placed in a high-temperature furnace for pre-calcination at 1230°C for 3 hours to form a main crystal phase powder for standby use;

[0071] Step 3: The pre-sintered powder is ball-milled, dried, granulated and sieved in sequence to obtain powder particles for pressing ceramics;

[0072] In step 3 and step 4, the ball milling time is 12 hours; the drying time is 2 hours, and the drying temperature is 120°C; the sintered powder is sieved through a 120-mesh sieve; granulation and sieving are performed by dropping an appropriate amount of 6wt% PVA adhesive into the powder, mixing it thoroughly, and sieving it through a 60-mesh sieve;

[0073] Step 4: Press the powder particles into a ceramic green body under a pressure of 12 MPa, sinter the ceramic green body in a high-temperature furnace, heat it from room temperature to 600°C at 5°C / min, and keep it at 120°C for debinding, continue to heat it to 1420°C and keep it at that temperature for 4 hours, and then cool it to 700°C at 3°C / min until it cools to room temperature;

[0074] Step 5: Polish, grind and clean the ceramic sample sintered in step 4, evenly coat the front and back sides of the sample with silver electrode slurry, and heat it at 600°C for 30 minutes to obtain a high entropy perovskite ceramic sample.

[0075] Embodiment 4:

[0076] Step 1: Prepare the ingredients according to the reaction equation and the required quantity of the required drug, using Na 2 CO 3 、SrCO 3 、TiO 2 、BaCO 3 SnO 2 , Nb2 O 5 、CaCO 3 、Bi 2 O 3 , Y 2 O 3 and ZrO 2 As raw materials, the molar ratio is 1:4:4:4:4:1:4:1:4, and 2% mol of Na 2 CO 3 , 2% mol Bi 2 O 3 A mixture A is obtained;

[0077] Step 2: The mixture A, zirconium spheroids and anhydrous ethanol are ball milled, dried and briquette-pressed in a mass ratio of 1:2:1, and then placed in a high-temperature furnace for pre-calcination at a temperature of 1210°C for 3 hours to form a main crystal phase powder for standby use;

[0078] Step 3: The pre-sintered powder is ball-milled, dried, granulated and sieved in sequence to obtain powder particles for pressing ceramics;

[0079] In step 3 and step 4, the ball milling time is 12 hours; the drying time is 2 hours, and the drying temperature is 120°C; the sintered powder is sieved through a 120-mesh sieve; granulation and sieving are performed by dropping an appropriate amount of 6wt% PVA adhesive into the powder, mixing it thoroughly, and sieving it through a 60-mesh sieve;

[0080] Step 4: Press the powder particles into a ceramic green body under a pressure of 12 MPa, sinter the ceramic green body in a high-temperature furnace, heat it from room temperature to 600°C at a rate of 5°C / min, and keep it at that temperature for 120 minutes to debind, continue to heat it to 1410°C and keep it at that temperature for 4 hours, and then cool it down to 700°C at a rate of 3°C / min until it cools to room temperature;

[0081] Step 5: Polish, grind and clean the ceramic sample sintered in step 4, evenly coat the front and back sides of the sample with silver electrode slurry, and heat it at 600°C for 30 minutes to obtain a high entropy perovskite ceramic sample.

[0082] Embodiment 5:

[0083] Step 1: Prepare the ingredients according to the reaction equation and the required quantity of the required drug, using Na 2 CO 3 、SrCO 3 、TiO 2 、BaCO 3 SnO 2 , Nb 2 O 5 、CaCO 3 、Bi 2 O 3, Y 2 O 3 and ZrO 2 As raw materials, the molar ratio is 1:4:4:4:4:1:4:1:4, and 3% mol of Na 2 CO 3 , 2% mol Bi 2 O 3 A mixture A is obtained;

[0084] Step 2: The mixture A, zirconium spheroids and anhydrous ethanol are ball milled, dried and briquette-pressed in a mass ratio of 1:2:1, and then placed in a high-temperature furnace for pre-calcination at 1220°C for 3 hours to form a main crystal phase powder for standby use;

[0085] Step 3: The pre-sintered powder is ball-milled, dried, granulated and sieved in sequence to obtain powder particles for pressing ceramics;

[0086] In step 3 and step 4, the ball milling time is 12 hours; the drying time is 2 hours, and the drying temperature is 120°C; the sintered powder is sieved through a 120-mesh sieve; granulation and sieving are performed by dropping an appropriate amount of 6wt% PVA adhesive into the powder, mixing it thoroughly, and sieving it through a 60-mesh sieve;

[0087] Step 4: Press the powder particles into a ceramic green body at a pressure of 12 MPa, sinter the ceramic green body in a high-temperature furnace, heat it from room temperature to 600°C at a rate of 5°C / min, and keep it at that temperature for 120 minutes to debind, continue to heat it to 1420°C and keep it at that temperature for 4 hours, and then cool it to 700°C at a rate of 3°C / min until it cools to room temperature;

[0088] Step 5: Polish, grind and clean the ceramic sample sintered in step 4, evenly apply silver electrode slurry on both sides of the sample, and keep it at 500-600° C. for 20-40 minutes to obtain a high entropy perovskite ceramic sample.

[0089] Embodiment 6:

[0090] Step 1: Prepare the ingredients according to the reaction equation and the required quantity of the required drug, using Na 2 CO 3 、SrCO 3 、TiO 2 、BaCO 3 SnO 2 , Nb 2 O 5 、CaCO 3 、Bi 2 O 3 , Y 2 O 3 and ZrO 2As raw materials, the molar ratio is 1:4:4:4:4:1:4:1:4, and 4% mol of Na 2 CO 3 , 2% mol Bi 2 O 3 A mixture A is obtained;

[0091] Step 2: The mixture A, zirconium spheroids and anhydrous ethanol are ball milled, dried and briquette-pressed in a mass ratio of 1:2:1, and then placed in a high-temperature furnace for pre-calcination at 1230°C for 3 hours to form a main crystal phase powder for standby use;

[0092] Step 3: The pre-sintered powder is ball-milled, dried, granulated and sieved in sequence to obtain powder particles for pressing ceramics;

[0093] In step 3 and step 4, the ball milling time is 12 hours; the drying time is 2 hours, and the drying temperature is 120°C; the sintered powder is sieved through a 120-mesh sieve; granulation and sieving are performed by dropping an appropriate amount of 6wt% PVA adhesive into the powder, mixing it thoroughly, and sieving it through a 60-mesh sieve;

[0094] Step 4: Press the powder particles into a ceramic green body at a pressure of 12 MPa, sinter the ceramic green body in a high-temperature furnace, heat it from room temperature to 600 ° C at 5 ° C / min, and keep it at this temperature for 120 minutes to debind, continue to heat it to 1430 ° C and keep it at this temperature for 4 hours, and then cool it to 700 ° C at 3 ° C / min until it cools to room temperature;

[0095] Step 5: Polish, grind and clean the ceramic sample sintered in step 4, evenly coat the front and back sides of the sample with silver electrode slurry, and heat it at 600°C for 30 minutes to obtain a high entropy perovskite ceramic sample.

[0096] Embodiment 7:

[0097] Step 1: Prepare the ingredients according to the reaction equation and the required quantity of the required drug, using Na 2 CO 3 、SrCO 3 、TiO 2 、BaCO 3 SnO 2 , Nb 2 O 5 、CaCO 3 、Bi 2 O 3 , Y 2 O 3 and ZrO 2 As raw materials, the molar ratio is 1:4:4:4:4:1:4:1:4, and 3% mol of Na 2 CO 3、3% mol Bi 2 O 3 A mixture A is obtained;

[0098] Step 2: The mixture A, zirconium spheroids and anhydrous ethanol are ball milled, dried and briquette-pressed in a mass ratio of 1:2:1, and then placed in a high-temperature furnace for pre-calcination at a temperature of 1210°C for 3 hours to form a main crystal phase powder for standby use;

[0099] Step 3: The pre-sintered powder is ball-milled, dried, granulated and sieved in sequence to obtain powder particles for pressing ceramics;

[0100] In step 3 and step 4, the ball milling time is 12 hours; the drying time is 2 hours, and the drying temperature is 120°C; the sintered powder is sieved through a 120-mesh sieve; granulation and sieving are performed by dropping an appropriate amount of 6wt% PVA adhesive into the powder, mixing it thoroughly, and sieving it through a 60-mesh sieve;

[0101] Step 4: Press the powder particles into a ceramic green body at a pressure of 12 MPa, sinter the ceramic green body in a high-temperature furnace, heat it from room temperature to 600 ° C at 5 ° C / min, and keep it at this temperature for 120 minutes to debind, continue to heat it to 1430 ° C and keep it at this temperature for 4 hours, and then cool it to 700 ° C at 3 ° C / min until it cools to room temperature;

[0102] Step 5: Polish, grind and clean the ceramic sample sintered in step 4, evenly coat the front and back sides of the sample with silver electrode slurry, and heat it at 600°C for 30 minutes to obtain a high entropy perovskite ceramic sample.

[0103] Embodiment 8:

[0104] Step 1: Prepare the ingredients according to the reaction equation and the required quantity of the required drug, using Na 2 CO 3 、SrCO 3 、TiO 2 、BaCO 3 SnO 2 , Nb 2 O 5 、CaCO 3 、Bi 2 O 3 , Y 2 O 3 and ZrO 2 As raw materials, the molar ratio is 1:4:4:4:4:1:4:1:4, and 4% mol of Na 2 CO 3 、3% mol Bi 2 O 3 A mixture A is obtained;

[0105] Step 2: The mixture A, zirconium spheroids and anhydrous ethanol are ball milled, dried and briquette-pressed in a mass ratio of 1:2:1, and then placed in a high-temperature furnace for pre-calcination at 1220°C for 3 hours to form a main crystal phase powder for standby use;

[0106] Step 3: The pre-sintered powder is ball-milled, dried, granulated and sieved in sequence to obtain powder particles for pressing ceramics;

[0107] In step 3 and step 4, the ball milling time is 12 hours; the drying time is 2 hours, and the drying temperature is 120°C; the sintered powder is sieved through a 120-mesh sieve; granulation and sieving are performed by dropping an appropriate amount of 6wt% PVA adhesive into the powder, mixing it thoroughly, and sieving it through a 60-mesh sieve;

[0108] Step 4: Press the powder particles into a ceramic green body under a pressure of 12 MPa, sinter the ceramic green body in a high-temperature furnace, heat it from room temperature to 600°C at a rate of 5°C / min, and keep it at that temperature for 120 minutes to debind, continue to heat it to 1440°C and keep it at that temperature for 4 hours, and then cool it down to 700°C at a rate of 3°C / min until it cools to room temperature;

[0109] Step 5: Polish, grind and clean the ceramic sample sintered in step 4, evenly coat the front and back sides of the sample with silver electrode slurry, and heat it at 600°C for 30 minutes to obtain a high entropy perovskite ceramic sample.

[0110] Embodiment 9:

[0111] Step 1: Prepare the ingredients according to the reaction equation and the required quantity of the required drug, using Na 2 CO 3 、SrCO 3 、TiO 2 、BaCO 3 SnO 2 , Nb 2 O 5 、CaCO 3 、Bi 2 O 3 , Y 2 O 3 and ZrO 2 As raw materials, the molar ratio is 1:4:4:4:4:1:4:1:4, and 5% mol of Na 2 CO 3 、3% mol Bi 2 O 3 A mixture A is obtained;

[0112] Step 2: The mixture A, zirconium spheroids and anhydrous ethanol are ball milled, dried and briquette-pressed in a mass ratio of 1:2:1, and then placed in a high-temperature furnace for pre-calcination at 1230°C for 3 hours to form a main crystal phase powder for standby use;

[0113] Step 3: The pre-sintered powder is ball-milled, dried, granulated and sieved in sequence to obtain powder particles for pressing ceramics;

[0114] In step 3 and step 4, the ball milling time is 12 hours; the drying time is 2 hours, and the drying temperature is 120°C; the sintered powder is sieved through a 120-mesh sieve; granulation and sieving are performed by dropping an appropriate amount of 6wt% PVA adhesive into the powder, mixing it thoroughly, and sieving it through a 60-mesh sieve;

[0115] Step 4: Press the powder particles into a ceramic green body at a pressure of 12 MPa, sinter the ceramic green body in a high-temperature furnace, heat it from room temperature to 600 ° C at 5 ° C / min, and keep it at this temperature for 120 minutes to debind, continue to heat it to 1450 ° C and keep it at this temperature for 4 hours, and then cool it to 700 ° C at 3 ° C / min until it cools to room temperature;

[0116] Step 5: Polish, grind and clean the ceramic sample sintered in step 4, evenly coat the front and back sides of the sample with silver electrode slurry, and heat it at 600°C for 30 minutes to obtain a high entropy perovskite ceramic sample.

[0117] The experimental results show that at low temperature (1400-1420℃) Na 2 CO 3 、Bi 2 O 3 The optimal doping amount is 3 mol and 1 mol, corresponding to Example 3; at medium temperature (1410-1430°C), Na 2 CO 3 、Bi 2 O 3 The optimal doping amount is 4 mol and 2 mol, corresponding to Example 6; at high temperature (1430-1450°C), Na 2 CO 3 、Bi 2 O 3 The optimal doping amount is 4 mol and 3 mol, corresponding to Example 8. Figures 2 to 7 It can be seen that the prepared samples have small grains as a whole, a dense microstructure, clear grain boundaries and almost invisible pores, but it can be clearly seen that Example 3 has the smallest submicron grain size. Figure 3 , Figure 5 and Figure 7From the average grain distribution diagram, it can be seen that the grain sizes of Example 3, Example 6, and Example 8 are 0.34um, 0.63um, and 0.78um, respectively, which is conducive to achieving a high breakdown field strength. Example 3 has the smallest submicron grain size, so its electrical properties are further tested. Figure 8 The PE rings of the sample of Example 3 tested under different electric fields are shown. It can be seen that the ceramic obtains a breakdown field strength of 460 kV / cm, and it can also be observed that the PE curve shows a linear trend.

[0118] Fig. 9 The corresponding energy storage characteristics were calculated and plotted. The efficiency of all field strength samples was above 80% (84.83% to 96.59%). As the field strength increased, the recoverable energy density gradually increased. At the highest electric field of 460 kV / cm, the ceramic obtained 1.4296 J / cm 3 The highest Wrec and high energy efficiency of 84.83%. The high entropy perovskite ceramic material with submicron fine grain structure prepared by the present invention adopts the conventional solid phase method and normal pressure sintering. Not only is the preparation process simple and easy to operate, the cost of the required materials is low, but also it has submicron ultrafine grain size, high breakdown field strength and good energy efficiency. The high entropy strategy breaks the conventional material design concept and provides a new idea for the design of dielectric ceramic materials.

[0119] The high-entropy perovskite ceramic material with a submicron fine-grained structure and the preparation method thereof proposed in the present invention have the following advantages:

[0120] 1) The present invention adopts a solid phase method for preparation, which has simple steps, low material cost, mature technology, and is suitable for mass production. 2) In the sintering process of the ceramic material, the present invention takes into account the Na 2 CO 3 、Bi 2 O 3 The influence of volatilization on the phase structure of high entropy perovskite ceramic materials is studied, and the optimal doping amount is explored by overdoping. The experimental results are more convincing. 3) The high entropy perovskite ceramic material with an ultrafine grain structure proposed in the present invention has a submicron microstructure with extremely small grain size, and the grains are tightly combined with almost no obvious gaps, and has good compactness. 4) Small grain size is conducive to the improvement of the breakdown field strength in ceramics, and it is easier to obtain large recoverable energy density and efficiency.

[0121] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A high entropy perovskite ceramic material with a submicron fine-grained structure, characterized in that: The chemical composition of high entropy perovskite ceramic materials is (Na 1 / 8 Ba 1 / 4 Ca 1 / 4 Sr 1 / 4 Bi 1 / 8 )(Y 1 / 8 Zr 1 / 4 Sn 1 / 4 Ti 1 / 4 Nb 1 / 8 )O3, with a microscopic grain structure.

2. A method for preparing a high-entropy perovskite ceramic material with a submicron fine-grained structure according to claim 1, characterized in that: The following steps are involved: Step 1: Mix Na2CO3, SrCO3, TiO2, BaCO3, SnO2, Nb2O5, CaCO3, Bi2O3, Y2O3 and ZrO2 to obtain a mixture A; Step 2: ball milling, drying and briquetting the mixture A in sequence, and then pre-sintering to form a main crystal phase powder; Step 3, the pre-sintered main crystal phase powder is subjected to ball milling, drying, granulation and sieving in sequence to obtain powder particles; Step 4: Pressing the powder particles into a ceramic green body, sintering until cooled to room temperature, and obtaining a high entropy perovskite ceramic material; In step 2, the ball milling time is 12 hours; the drying time is 1 hour to 2 hours, and the drying temperature is 100°C to 120°C; the pre-calcining time is 3 hours to 4 hours, and the pre-calcining temperature is 1200°C to 1240°C; In step 2, zirconium spheroids and anhydrous ethanol are added to mixture A during ball milling, and mixture A, zirconium spheroids and anhydrous ethanol are mixed in a mass ratio of 1:2:

1.

3. The method for preparing a high-entropy perovskite ceramic material with a submicron fine-grained structure according to claim 2, characterized in that: In step 1, the molar ratio of Na2CO3, SrCO3, TiO2, BaCO3, SnO2, Nb2O5, CaCO3, Bi2O3, Y2O3 and ZrO2 is 1:4:4:4:4:1:4:1:4, and 1%-5mol% NaCO3 and Bi2O3 are doped to obtain mixture A.

4. The method for preparing a high-entropy perovskite ceramic material with a submicron fine-grained structure according to claim 2, characterized in that: In step 3, the pre-calcined powder is first ground into fine powder and passed through a 120-mesh sieve, and then ball milled.

5. The method for preparing a high-entropy perovskite ceramic material with a submicron fine-grained structure according to claim 2, characterized in that: In step three, granulation and sieving are performed by slowly dropping an appropriate amount of a binder with a concentration of 4wt% to 6wt% with a dropper during the grinding process of the powder, and sieving with a 60-mesh sieve to obtain a uniform powder.

6. The method for preparing a high-entropy perovskite ceramic material with a submicron fine-grained structure according to claim 5, characterized in that: In step three, the binder is a polyvinyl alcohol solution.

7. The method for preparing a high-entropy perovskite ceramic material with a submicron fine-grained structure according to claim 2, characterized in that: In step 4, the granulated powder particles are pressed into a ceramic green body at a pressure of 8MPa to 12MPa.

8. The method for preparing a high-entropy perovskite ceramic material with a submicron fine-grained structure according to claim 2, characterized in that: In step four, the ceramic green body is sintered, the temperature is increased from room temperature to 500°C~600°C at a rate of 3°C / min~5°C / min, and the temperature is kept for 120min~140min for debinding, the temperature is further increased to 1400°C~1450°C and kept for 3h~4h, and then the temperature is decreased to 600°C~700°C at a rate of 3°C / min~5°C / min until it is cooled to room temperature to obtain a high entropy perovskite ceramic material.