A damage initiation characterization method for coupled failure behavior of heterogeneous adhesive joints
By constructing an extended power index damage criterion model and experiment to obtain fracture strength parameters, combined with simulation simulation, the simulation accuracy problem caused by the complexity of the glue joint failure mode in the existing technology is solved, and the precise failure of the heterogeneous glue joint is achieved Behavioral judgment.
Patent Information
- Application Number
- CN202310767081.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-27
AI Technical Summary
The damage criterion model of glued joints in existing simulation simulations fails to effectively consider the multiple failure modes of the joints, resulting in poor simulation calculation accuracy and it is difficult to accurately characterize the coupling failure behavior of heterogeneous glued joints.
Build a extended power index damage criterion model, and obtain fracture strength parameters and power index parameters by preparing different types of samples and performing tensile and shear strength tests. Combined with simulation, we can judge whether the heterogeneous glue joints begin to fail. .
The ability to accurately judge the failure behavior in the simulation of heteroglobin joints is realized, and the simulation calculation accuracy is improved.
Smart Images

Figure CN117012309B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to damage failure analysis of adhesive joints, and in particular to a damage initialization characterization method for coupled failure behavior of heterogeneous adhesive joints. Background Art
[0002] At present, the structure of automobile bodies adopts a multi-material structure, including high-strength steel, lightweight alloy materials and fiber-reinforced composite materials. The connection methods of multi-materials include welding, riveting, gluing, etc. Among them, the gluing process can connect various identical or different materials, and the process is simple and the production efficiency is high. The stress distribution of the adhesive joint is uniform, the fatigue strength is high and the service life is long. The entire adhesive surface can withstand the load and has good sealing, insulation, heat insulation, moisture-proof and shock-absorbing functions. However, in practice, the failure modes of adhesive joints are complex and diverse. The damage criterion model of adhesive joints in existing simulations does not take into account the multiple failure modes of the joints, and it is difficult to accurately characterize the coupled failure behavior of adhesive joints, resulting in poor simulation calculation accuracy. Summary of the invention
[0003] In view of the deficiencies in the prior art, the present invention provides a method for characterizing the initial damage of the coupled failure behavior of heterogeneous adhesive joints, which is used to determine whether the heterogeneous adhesive joints begin to fail.
[0004] The present invention achieves the above technical objectives through the following technical means.
[0005] A damage initiation characterization method for coupled failure behavior of heterogeneous adhesive joints, characterized by:
[0006] (1) Construct an extended power exponential damage criterion model for coupled failure of adhesive joints:
[0007]
[0008] Where: interAIC , σ interAIIC , σ interAIIIC are the stress values of type I, type II and type III fracture forms of the interface failure between the adhesive and the base material A, σ interBIC , σ interBIIC , σ interBIIIC are the stress values of type I, type II and type III fracture forms of the interface failure between the adhesive and the base material B, σ GlueIC , σ GlueIIC , σ GlueIIIC are the stress values of type I, type II and type III fracture forms of the adhesive failure, σ interAI , σ interAII , σ interAIII are the strength values of type I, type II and type III fracture modes of the interface failure between the adhesive and the base material A when they exist separately, σinterBI , σ interBII , σ interBIII are the strength values of type I, type II and type III fracture modes of the interface failure between the adhesive and the base material B when they exist separately, σ GlueI , σ GlueII , σ GlueIII are the strength values of type I, type II and type III fracture modes of adhesive failure when they exist alone, respectively; the power exponents α1 and β1 represent the coupling effects of the three different fracture modes on its fracture behavior when the interface between adhesive and base material A fails; the power exponents α2 and β2 represent the coupling effects of the three different fracture modes on its fracture behavior when the interface between adhesive and base material B fails; the power exponents α3 and β3 represent the coupling effects of the three different fracture modes on its fracture behavior when the adhesive fails itself;
[0009] (2) Prepare butt joint specimens and shear specimens with cohesive failure of the adhesive layer, and conduct tensile and shear strength tests respectively. The average fracture strength of the test data is taken as σ GlueI , σ GlueII , σ GlueIII ;
[0010] Cross tensile specimens and single lap specimens with interface failure on the A side of the parent material were prepared, and tensile and shear strength tests were performed respectively. The average fracture strength of the test data was taken as σ interAI , σ interAII , σ interAIII ;
[0011] Cross tensile specimens and single lap specimens with interface failure on the B side of the parent material were prepared, and tensile and shear strength tests were performed respectively. The average fracture strength of the test data was taken as σ interBI , σ interBII , σ interBIII ;
[0012] (3) Prepare single lap joint specimens of variable thickness base material A and constant thickness base material B with three different slopes, and conduct 30° tension-shear coupling test and 60° tension-shear coupling test respectively; obtain the force-displacement curve of each group of experiments from the experimental data and calculate the corresponding fracture strength value, simulate each group of experimental conditions, and perform error analysis between the fracture strength value calculated by the simulation result curve and the fracture strength value obtained by the experiment through the update and iteration of the power exponent. When RSME is less than 0.05, the accuracy requirement is met, and the power exponent of the simulation is the power exponent parameter calculated;
[0013] (4) The determined σ GlueI , σ GlueII , σ GlueIII , σ interAI , σ interAII , σ interAIII , σ interBI , σinterBII , σ interBIII The sum power exponent is substituted into formula (1) and used as the fracture strength model in the constitutive model of the adhesive in the simulation of heterogeneous adhesive joints to determine whether the heterogeneous adhesive joints begin to fail.
[0014] Furthermore, the device for preparing the butt joint specimen of cohesive failure of the adhesive layer includes a front plate of tooling 1, a rear plate of tooling 1, a bottom plate of tooling 1 and a feed screw of tooling 1; the bottom plate of tooling 1 is stepped, the bottom of the front plate of tooling 1 is installed at the higher end of the step, and the bottom of the rear plate of tooling 1 is installed at the lower end of the step; a groove for placing the specimen is provided on the lower end of the step of the bottom plate of tooling 1; and the feed screw of tooling 1 is installed on the front plate of tooling 1.
[0015] Furthermore, the device for preparing shear specimens of cohesive failure of the adhesive layer includes a front plate of tooling 2, a rear plate of tooling 2, a bottom plate of tooling 2, a pressure plate of tooling 2 and a feed screw of tooling 2; the bottom plate of tooling 2 is stepped, the bottom of the front plate of tooling 2 is installed at the higher end of the step, and the bottom of the rear plate of tooling 2 is installed at the lower end of the step; the pressure plate of tooling 2 is placed between the front plate of tooling 2 and the rear plate of tooling 2, and is located on the lower level of the step; the feed screw of tooling 2 is installed on the front plate of tooling 2; a limiting boss is provided in the middle of the bottom plate of tooling 2 for lateral positioning of the shear specimen.
[0016] Furthermore, the device for preparing the cross tensile specimen includes a front plate of tooling 3, a rear plate of tooling 3, a connecting plate of tooling 3, a pressure plate of tooling 3 and a feed screw of tooling 3; the connecting plate of tooling 3 is in a "C" shape, and the horizontal plane is stepped, the lower part of the front plate of tooling 3 is connected to the higher side of the step of the connecting plate of tooling 3, and the lower part of the rear plate of tooling 3 is connected to the lower side of the step of the connecting plate of tooling 3; the pressure plate of tooling 3 is in an inverted "convex" shape, placed between the front plate of tooling 3 and the rear plate of tooling 3, and located on the lower level of the step; the feed screw of tooling 3 is installed on the front plate of tooling 3; the pressure plate of tooling 3 is provided with a groove on the horizontal plane perpendicular to the direction of the feed screw, and the rear plate of tooling 3 is also provided with a groove on the vertical plane perpendicular to the direction of the feed screw, for placing the specimen.
[0017] Furthermore, the device for preparing a single lap specimen comprises a front plate of tooling 4, a rear plate of tooling 4, a bottom plate of tooling 4, a pressure plate of tooling 4 and a feed screw of tooling 4; the bottom plate of tooling 4 is stepped, the bottom of the front plate of tooling 4 is installed at the higher end of the step, and the bottom of the rear plate of tooling 4 is installed at the lower end of the step; the pressure plate of tooling 4 is located between the front plate of tooling 4 and the rear plate of tooling 4, and is located on the lower level of the step; the feed screw of tooling 4 is installed on the front plate of tooling 4; the pressure plate of tooling 4 and the rear plate of tooling 4 are both designed with grooves for placing specimens and gaskets in the horizontal plane perpendicular to the direction of the feed screw, and the grooves on both sides are rotationally symmetrical.
[0018] Furthermore, in (2), during the preparation of the bonding specimen, cracks are preformed by laying a polytetrafluoroethylene film to guide the crack propagation of the bonding specimen.
[0019] Furthermore, in (2), when preparing the sample, it is necessary to apply adhesive on the sample, and select the adhesive layer control gasket according to the thickness of the adhesive layer, wherein: when preparing the butt joint sample with cohesive failure of the adhesive layer, the thickness of the adhesive layer T glue1 Control the thickness of the gasket T with the glue layer shim Satisfaction: T glue1 =T shim -T boss1 -T boss2 , where T boss1 is the height of the butt-jointed specimen boss at one end, T boss2 is the height of the butt specimen boss at the other end; when preparing shear specimens for cohesive failure of the adhesive layer, the adhesive layer thickness T glue2 Control the thickness of the gasket T with the glue layer shim Satisfaction: T glue2 =T Loading +T shim -T Bonding1 -T Bonding2 , where T Loading is the width of the specimen loading end, T Bonding1 T is the width of the bonding end of the shear specimen at one end. Bonding2 is the width of the bonding end of the shear specimen at the other end; when preparing the cross tensile specimen, the thickness of the adhesive layer T glue3 Control the thickness of the gasket T with the glue layer shim Satisfaction: T glue3 =T shim +2*T groove -T sample , where T groove T is the depth of the grooves pre-cut between the pressure plate and the back plate. sample is the thickness of the cross tensile specimen; when preparing a single lap specimen, the adhesive layer thickness T glue4 Control the thickness of the gasket T with the glue layer shim Satisfaction: T glue4 =T shim +2*T groove -T' sample , where T groove Depth of the grooves pre-cut between the pressure plate and the back plate, T' sample is the thickness of the single lap specimen.
[0020] Furthermore, when the butt joint specimen with cohesive failure in the adhesive layer is subjected to tensile and shear strength tests, the butt joint specimen needs to be equipped with a common tension and shearing fixture. The upper end of the common tension and shearing fixture is a clamping end clamped with a testing machine, and the lower connecting end is provided with a space for placing the specimen. During the test, the butt joint specimen and the common tension and shearing fixture are assembled by a pin.
[0021] Furthermore, when the cross tensile specimen with failed interface on the A / B side of the base material is subjected to a tensile strength test, a T-shaped test fixture is provided, the upper end of the fixture is a clamping end connected to a universal tensile testing machine, and the lower end is fixed to the specimen.
[0022] Furthermore, when the single lap specimen is subjected to the tension-shear coupling test, an arc-shaped fixture is provided, and the fixture and the specimen assembly end form angles of 30° and 60° with the axis of the testing machine, and the specimen clamping end is assembled with the fixture.
[0023] The beneficial effects of the present invention are:
[0024] The butt joint specimens, shear specimens, cross tensile specimens and single lap specimens used in the test of the present invention are designed with their own preparation devices according to the characteristics of the specimens; and in the process of preparing the adhesive specimens, cracks are prefabricated by laying polytetrafluoroethylene films to guide the crack propagation of the adhesive specimens and realize different failure modes; in addition, the thickness of the specimen adhesive layer is controlled by gaskets, and the thickness of the adhesive layer of the adhesive specimen can be accurately controlled by selecting gaskets of appropriate thickness according to the requirements of the adhesive layer thickness when the thickness of the parent material is different. The extended power exponential damage criterion model of the present invention can accurately determine whether the heterogeneous adhesive joint begins to fail in the simulation of heterogeneous adhesive joints. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] FIG1( a ) is a schematic diagram of a type I fracture form of an adhesive joint according to the present invention;
[0026] FIG1( b ) is a schematic diagram of the type II fracture form of the adhesive joint according to the present invention;
[0027] FIG1( c ) is a schematic diagram of the type III fracture form of the adhesive joint according to the present invention;
[0028] FIG2( a ) is a schematic diagram of the butt joint specimen and test loading according to the present invention;
[0029] FIG2( b ) is a schematic diagram of the shear specimen and test loading according to the present invention;
[0030] FIG2( c ) is a schematic diagram of the cross tensile specimen and test loading according to the present invention;
[0031] FIG2( d ) is a schematic diagram of the single lap joint specimen and test loading according to the present invention;
[0032] Figure 3 Schematic diagram of the parent materials with three slopes according to the present invention;
[0033] FIG4( a ) is a schematic diagram of a 30° offset tension-shear coupling test according to the present invention;
[0034] FIG4( b ) is a schematic diagram of a 60° offset tension-shear coupling test according to the present invention;
[0035] Figure 5 This is a schematic diagram of the structure of the docking sample preparation device of the present invention;
[0036] Figure 6 This is a schematic diagram of the structure of the shear specimen preparation device of the present invention;
[0037] FIG. 7( a ) is a schematic structural diagram of a cross tensile specimen preparation device according to the present invention;
[0038] FIG7( b ) is a schematic diagram of the interior of the cross tensile specimen preparation device of the present invention;
[0039] FIG. 7( c ) is a second schematic diagram of the interior of the cross tensile specimen preparation device of the present invention;
[0040] FIG8( a ) is a schematic structural diagram of a single-lap specimen preparation device according to the present invention;
[0041] FIG8( b ) is a schematic diagram of the interior of the single-lap specimen preparation device of the present invention;
[0042] FIG8( c ) is a second schematic diagram of the interior of the single lap specimen preparation device of the present invention;
[0043] Fig. 9 This is a schematic diagram of the structure of the common clamp for pulling and shearing of the present invention;
[0044] Fig.10 This is a schematic diagram of the structure of the cross tensile test fixture of the present invention;
[0045] Fig.11 This is a schematic diagram of the structure of the tension-shear coupling test fixture of the present invention;
[0046] Fig.12 It is a flow chart of the damage initial characterization method of the coupled failure behavior of heterogeneous adhesive joints according to the present invention;
[0047] In the figure: 1- docking specimen preparation device, 101- tooling 1 front plate, 102- tooling 1 rear plate, 103- tooling 1 bottom plate, 104- tooling 1 feed screw, 2- shear specimen preparation device, 201- tooling 2 front plate, 202- tooling 2 rear plate, 203- tooling 2 bottom plate, 204- tooling 2 pressure plate, 205- tooling 2 feed screw, 3- cross tensile specimen preparation device, 301- tooling 3 front plate, 302- tooling 3 rear plate, 303- tooling 3 connecting plate, 304- tooling 3 pressure plate, 305- tooling 3 feed screw, 4- single lap specimen preparation device, 401- tooling 4 front plate, 402- tooling 4 rear plate, 403- tooling 4 bottom plate, 404- tooling 4 pressure plate, 405- tooling 4 feed screw. DETAILED DESCRIPTION
[0048] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited thereto.
[0049] A damage initiation characterization method for coupled failure behavior of heterogeneous adhesive joints specifically comprises the following steps:
[0050] 1. Extended power exponential damage criterion model for coupled failure of adhesive joints
[0051] When a heterogeneous adhesive joint fractures, it often manifests not only a single failure mode, but multiple failure modes are coupled. However, the fracture strength under each failure mode is different, and the fracture strength of various failure modes needs to be considered in the damage criterion model. In order to accurately and efficiently determine the damage initiation of multiple failure modes coupling in heterogeneous adhesive joints, the power exponential nominal stress damage criterion model that considers the coupling of type I, type II and type III fracture forms is expanded to a damage criterion model that couples all fracture forms of the three failure modes (each failure mode contains three fracture forms), in which the power exponential parameter is variable and used to describe the coupling effect between various fracture forms. The following mathematical form of the coupled failure damage criterion model is constructed to determine the damage initiation:
[0052]
[0053] In the formula, σ interAIC , σ interAIIC , σ interAIIIC are the stress values of type I, type II and type III fracture forms of the interface failure between the adhesive and the base material A, σ interBIC , σ interBIIC , σ interBIIIC are the stress values of type I, type II and type III fracture forms of the interface failure between the adhesive and the base material B, σ GlueIC , σ GlueIIC , σ GlueIIIC are the stress values of type I, type II and type III fracture forms of the rubber failure; σ in the denominator interAI , σ interAII , σ interAIII are the strength values of type I, type II and type III fracture modes of the interface failure between the adhesive and the base material A when they exist separately, σ interBI , σ interBII , σ interBIII are the strength values of type I, type II and type III fracture modes of the interface failure between the adhesive and the base material B when they exist separately, σ GlueI , σ GlueII , σ GlueIIIThey are the strength values of type I, type II and type III fracture forms of adhesive failure when they exist alone. The power exponents α1 and β1 represent the coupling effects of the three different fracture forms on the fracture behavior of the adhesive and base material A under interface failure, the power exponents α2 and β2 represent the coupling effects of the three different fracture forms on the fracture behavior of the adhesive and base material B under interface failure, and the power exponents α3 and β3 represent the coupling effects of the three different fracture forms on the fracture behavior of the adhesive under self-failure. The power exponents (α1, β1, α2, β2, α3, β3) of each item are obtained by simulation curve fitting of the test results of type I and type II fracture strength of the coupled failure mode to inversely obtain the parameters.
[0054] The above-mentioned type I, type II and type III fracture forms are shown in Figure 1 (a), (b), (c), which are opening type (type I), sliding type (type II) and tearing type (type III), respectively. The type II and type III fracture forms of the adhesive joints show shear in different directions, while the adhesive area is the same. Therefore, it is believed that the strength values of type II and type III fracture forms are the same when they exist alone, that is, σ interBII =σ interBIII , σ GlueII =σ GlueIII The present invention obtains the type I fracture strength through tensile tests on butt specimens and cross tensile specimens, and the corresponding specimens and their test schematics are shown in Figures 2(a) and (c). The type II and type III fracture strengths are obtained through tensile shear tests on shear specimens and single lap specimens, and the corresponding specimens and their test schematics are shown in Figures 2(b) and (d).
[0055] 2. Parameter acquisition test plan
[0056] All the required experiments are shown in Table 1 below. The specimens with a single failure mode in the table were subjected to tensile strength tests and shear strength tests respectively and repeated three times. The test results were collated to obtain the fracture strength parameter (i.e., the denominator in formula (1)) in the extended power exponential damage criterion model. The specimens with three slopes and multiple failure modes coupled were subjected to a 30° offset and a 60° offset tensile-shear coupling test respectively, and the power exponential parameters in the damage criterion model were inversely calculated by simulating and fitting the test curves. The parent materials with three slopes are shown in Figure 1. Figure 3 As shown, the tension-shear coupling test is shown in Figure 4(a) and (b).
[0057] Table 1 Parameter acquisition test plan
[0058]
[0059]
[0060] 3. Fracture strength parameter acquisition process
[0061] Step (1): Preparation of samples for obtaining fracture strength parameters
[0062] In order to obtain a specific failure mode, it is necessary to lay a certain length of polytetrafluoroethylene film at the corresponding position during the preparation of the bonding specimen to pre-create cracks, which is used to guide the crack propagation of the bonding specimen, thereby inducing corresponding failure in the test through the pre-created cracks.
[0063] 1) Preparation of butt joint specimens for cohesive failure of adhesive layer
[0064] The butt joint specimen is a rectangular metal adhesive specimen. The butt joint specimen with cohesive failure of the adhesive layer is shown in Figure 2(a). Specifically, the material should be a metal material with small deformation during the test, and the corresponding width and length dimensions should be selected according to the bonding area. The bonding end of the specimen is designed with a boss for placing a gasket, which can also serve to overflow the excess glue. The specimen is designed with a through hole at the loading end for cooperation with the pin of the tensile test fixture.
[0065] In order to more accurately prepare butt joint specimens with cohesive failure of the adhesive layer, the present invention designs and manufactures a butt joint specimen preparation device for accurately customizing the cohesive failure of the adhesive layer, such as Figure 5 As shown. The sample preparation device is a tool 1, which includes a front plate 101, a rear plate 102, a bottom plate 103 and a feed screw 104. The front plate 101 and the bottom of the rear plate 102 are connected to the two ends of the bottom plate 103 by bolts. The bottom plate 103 is stepped, the front plate 101 is installed on the higher step, and the rear plate 102 is installed on the lower step. The bottom plate 103 is designed with a groove, the groove width (in the horizontal plane perpendicular to the direction of the feed screw) is consistent with the width of the docking sample, and bosses are also provided at both ends of the groove width. The front plate 101 of the tool 1 is provided with a threaded hole, and the feed screw 104 of the tool 1 is installed and fixed through the threaded hole.
[0066] Furthermore, the steps for preparing the butt joint specimen with cohesive failure of the adhesive layer are as follows:
[0067] a. To achieve cohesive failure of the adhesive layer, the convex surface of the butt joint specimen should be evenly coated with sufficient adhesive. After coating, a polytetrafluoroethylene film of a certain width should be laid around the bonding end of the butt joint specimen and fixed on the butt joint specimen with transparent tape;
[0068] b. Apply an appropriate amount of anti-stick grease to the groove area of the bottom plate, place the butt joint specimen in the groove, and place adhesive layer control gaskets (gasket thickness is T) on both sides of the boss. shim ) to control the thickness of the adhesive layer. Different adhesive layer thicknesses can be achieved by selecting adhesive layer control gaskets of different thicknesses. The adhesive layer thickness is T glue1 =T shim -T boss1 -Tboss2 , where T boss1 is the height of the butt-jointed specimen boss at one end, T boss2 The height of the boss of the docking specimen at the other end;
[0069] c. Use a torque wrench to evenly rotate the feed screw to push the butt joint specimen and apply a pre-tightening force to achieve bonding of the butt joint specimen;
[0070] d. Fix the feed screw and send the tooling into the constant temperature box for adhesive curing. After the curing is completed, disassemble the tooling, take out the butt joint specimen, remove the overflowed glue and pull out the polytetrafluoroethylene film to prepare the butt joint specimen with cohesive failure of the glue layer.
[0071] 2) Preparation of shear specimens for cohesive failure of adhesive layer
[0072] The shear specimen is an L-shaped step specimen, and the shear specimen with cohesive failure of the adhesive layer is shown in Figure 2(b). The width of the bonding end of the specimen is smaller than the loading end of the specimen, and the shear specimen is designed with a through hole at the loading end to cooperate with the pin of the tensile test fixture.
[0073] In order to more accurately prepare the shear specimen of the cohesive failure of the adhesive layer, the present invention designs and manufactures a shear specimen preparation device for accurately customizing the cohesive failure of the adhesive layer, such as Figure 6 The sample preparation device is a tool 2, which includes a front plate 201 of tool 2, a rear plate 202 of tool 2, a bottom plate 203 of tool 2, a pressure plate 204 of tool 2, and a feed screw 205 of tool 2; the front plate 201 of tool 2 and the bottom of the rear plate 202 of tool 2 are connected to the two ends of the bottom plate 203 of tool 2 by bolts; the bottom plate 203 of tool 2 is stepped, and bosses are provided at both ends of the length direction of the bottom plate 203 of tool 2 (perpendicular to the feed screw direction on the horizontal plane); two limit bosses are also designed in the middle of the bottom plate 203 of tool 2 for lateral positioning of the shear sample, and a square through hole is designed in the middle for overflow of excess glue ; The front plate 201 of tooling 2 is installed on a higher level of the stairs, the rear plate 202 of tooling 2 is installed on a lower level of the stairs, and the pressure plate 204 of tooling 2 is placed between the front plate 201 of tooling 2 and the rear plate 202 of tooling 2, and is located on the lower level of the stairs; threaded holes are opened on the front plate 201 of tooling 2, and the feed screw 205 of tooling 2 is installed and fixed through the threaded holes; the width of the front plate 201 of tooling 2 and the rear plate 202 of tooling 2 (perpendicular to the feed screw direction in the horizontal plane) is consistent with the width of the bottom plate 203 of tooling 2, and the width of the pressure plate 204 of tooling 2 is smaller than the width of the front plate 201 of tooling 2 and the rear plate 202 of tooling 2.
[0074] Furthermore, the steps for preparing the shear specimen of the cohesive failure of the adhesive layer are as follows:
[0075] a. To achieve cohesive failure of the adhesive layer, the bonding surface of the shear specimen should be evenly coated with a sufficient amount of adhesive. After coating, a certain width of polytetrafluoroethylene film should be laid around the bonding end and fixed on the shear specimen with transparent tape;
[0076] b. Place the shear specimen in the groove of the bottom plate, and place adhesive layer control gaskets between the back plate and the specimen and between the pressure plate and the specimen to control the thickness of the adhesive layer. The thickness of the adhesive layer is T glue2 =T Loading +T shim -T Bonding1 -T Bonding2 , where T Loading is the width of the specimen loading end, T Bonding1 T is the width of the bonding end of the shear specimen at one end. Bonding2 The width of the bonding end of the shear specimen at the other end;
[0077] c. Use a torque wrench to evenly rotate the feed screw to push the shear specimen and apply a pre-tightening force to achieve bonding of the shear specimen;
[0078] d. Fix the feed screw and send the tooling into the constant temperature box for adhesive curing. After curing is completed, disassemble the tooling, take out the shear specimen, remove the overflowed glue and pull out the polytetrafluoroethylene film to prepare the shear specimen with cohesive failure of the glue layer.
[0079] 3) Preparation of cross tensile specimens with interface failure
[0080] The cross tensile specimen is a specimen made of homogeneous materials of equal thickness and bonded in a "cross" shape, as shown in Figure 2(c). Through holes are opened at both ends of the specimen for assembly with the cross tensile test fixture.
[0081] In order to more accurately prepare the cross tensile specimen of interface failure, the present invention designs and manufactures a device for preparing cross tensile specimens of interface failure with precision customization, as shown in Figures 7(a), (b), and (c). The specimen preparation device is a tooling 3, which includes a tooling 3 front plate 301, a tooling 3 rear plate 302, a tooling 3 connecting plate 303, a tooling 3 pressing plate 304, and a tooling 3 feed screw 305; the tooling 3 connecting plate 303 is in a "C" shape, and the horizontal plane of the tooling 3 connecting plate 303 is stepped. The lower parts of the tooling 3 front plate 301 and the tooling 3 rear plate 302 are provided with through holes that match the tooling 3 connecting plate 303. The lower part of the tooling 3 front plate 301 is connected to the tooling 3 connecting plate 303 by bolts. The tool 3 connecting plate 303 is connected at the higher side of the step, and the lower part of the tool 3 rear plate 302 is connected to the lower side of the step of the tool 3 connecting plate 303 by bolts; the tool 3 pressing plate 304 is in the shape of an inverted "convex" character, placed between the tool 3 front plate 301 and the tool 3 rear plate 302, and located on the lower level of the step of the tool 3 connecting plate 303; the width of the tool 3 front plate 301 and the tool 3 rear plate 302 (in the horizontal plane perpendicular to the direction of the feed screw) is ) is consistent with the width of the tool 3 connecting plate 303, the width of the tool 3 pressure plate 304 is smaller than the width of the tool 3 rear plate 302, and bosses are provided at both ends of the tool 3 pressure plate 304 in the length direction (parallel to the feed screw direction on the horizontal plane); 4 threaded holes are opened on the tool 3 front plate 301, and 4 tool 3 feed screws 305 are installed and fixed through the threaded holes; grooves consistent with the size of the cross tensile specimen are opened in the center of the opposite surfaces of the tool 3 pressure plate 304 and the tool 3 rear plate 302 (that is, the tool 3 pressure plate 304 is provided with a groove perpendicular to the feed screw direction on the horizontal plane, and the tool 3 rear plate 302 is provided with a groove perpendicular to the feed screw direction on the vertical plane), and the depth of the groove is lower than the thickness of the specimen; in addition, a sampling groove for convenient sampling is reserved at the upper end of the groove of the tool 3 rear plate 302, and a channel for convenient processing is reserved at the lower end; the tool 3 pressure plate 304 is provided with sampling grooves for convenient sampling and a channel for convenient processing on the left and right sides of the groove.
[0082] Furthermore, the steps for preparing the cross tensile specimen with interface failure are as follows:
[0083] a. Apply a proper amount of anti-sticking grease to the non-adhesive areas of the bottom plate, pressure plate and back plate grooves (except the area of the sample), place the sample in the pre-opened grooves of the pressure plate and back plate, and in order to achieve interface failure, lay a certain width of polytetrafluoroethylene film on the bonding area of one of the cross tensile specimens and fix it on the sample with transparent tape, and then evenly apply sufficient adhesive to the bonding area;
[0084] b. Select the appropriate thickness of the glue layer control gasket according to the thickness of the prepared sample glue layer. The thickness of the glue layer is T glue3 =T shim +2*T groove -T sample , where Tgroove T is the depth of the grooves pre-cut between the pressure plate and the back plate. sample is the thickness of the specimen;
[0085] c. Place the cross tensile test specimens in the grooves of the back plate and the pressure plate respectively, place the selected gaskets in the non-adhesive areas on both sides of the pressure plate and the back plate, place the pressure plate parallel to the back plate on the bottom plate and push it by hand until the two specimens on the pressure plate and the back plate are glued;
[0086] d. Keep your hand on the pressure plate and rotate the feed screw evenly to push the pressure plate to the gasket restraining position and apply preload force with a torque wrench;
[0087] e. Fix the feed screw and send the tooling into the constant temperature box for adhesive curing. After the curing is completed, disassemble the tooling, take out the sample, remove the overflowed glue and pull out the polytetrafluoroethylene film to prepare the cross tensile specimen with interface failure on the parent material side.
[0088] 4) Preparation of single lap joint specimens with interface failure
[0089] The single lap joint specimen is prepared by overlapping and gluing rectangular parent material samples, and a metal gasket with the same thickness as the parent material is bonded at the clamping end, as shown in Figure 2(d). In order to more accurately prepare single lap joint specimens with interface failure, the present invention designs and manufactures a single lap joint specimen preparation device for accurately customizing interface failure, as shown in Figures 8(a), (b), and (c). The sample preparation device is a tool 4, which includes a front plate 401, a rear plate 402, a bottom plate 403, a pressure plate 404 and a feed screw 405. The front plate 401 and the bottom of the rear plate 402 are connected to the bottom plate 403 by bolts. The bottom plate 403 is stepped, and the front plate 401 is installed on the higher level of the step, and the rear plate 402 is installed on the lower level of the step. The pressure plate 404 is placed between the front plate 401 and the rear plate 402, and is located on the lower level of the step. The width of the front plate 401 and the rear plate 402 (in the horizontal plane, perpendicular to the feed screw) of the tool 4 is 404. The width of the tool 4 bottom plate 403 is consistent with the width of the tool 4, the width of the tool 4 pressure plate 404 is smaller than the width of the tool 4 rear plate 402, and the tool 4 pressure plate 404 is designed with a groove for placing samples and gaskets in the horizontal plane perpendicular to the direction of the feed screw, and the depth of the groove is lower than the thickness of the sample; the tool 4 rear plate 402 is also designed with a groove for placing samples and gaskets, and the depth of the groove is lower than the thickness of the sample, and the arrangement position of the groove is rotationally symmetrical with the position of the groove on the tool 4 pressure plate 404; in addition, a sampling groove for convenient sampling is reserved at the upper end of the groove, and a channel for convenient processing is reserved at the lower end; a threaded hole is opened on the front plate 401 of the tool 4, and the feed screw 405 of the tool 4 is installed and fixed through the threaded hole.
[0090] Furthermore, the steps for preparing single lap tensile specimens with interface failure are as follows:
[0091] a. Apply a proper amount of anti-sticking grease to the non-adhesive areas of the bottom plate, pressure plate and back plate grooves (except the area of the sample), place the sample in the pre-opened grooves of the pressure plate and back plate, and in order to achieve interface failure, lay a certain width of polytetrafluoroethylene film in the bonding area of one of the single lap joint samples and fix it on the sample with transparent tape, and then evenly apply sufficient adhesive to the bonding area of the base material and the gasket;
[0092] b. Select the appropriate thickness of the glue layer control gasket according to the thickness of the glue layer of the prepared sample. The thickness of the glue layer is T glue4 =T shim +2*T groove -T' sample , where T groove Depth of the grooves pre-cut between the pressure plate and the back plate, T' sample is the thickness of the specimen;
[0093] c. Place the single lap joint specimens in the grooves of the back plate and the pressure plate, respectively, place the selected gaskets on the non-adhesive areas on both sides of the pressure plate and the back plate, place the pressure plate parallel to the back plate on the bottom plate and push it by hand until the two specimens on the pressure plate and the back plate are glued;
[0094] d. Keep your hand on the pressure plate and rotate the feed screw evenly to push the pressure plate to the gasket restraining position and apply preload force with a torque wrench;
[0095] e. Fix the feed screw and send the tooling into the constant temperature box for adhesive curing. After the curing is completed, disassemble the tooling, take out the sample, remove the overflowed glue and pull out the polytetrafluoroethylene film to prepare the single lap joint sample with interface failure on the parent material side.
[0096] Step (2): Fracture strength parameter acquisition test
[0097] Type I and Type II strength tests were performed on the specimens with three different failure modes to obtain six fracture strength parameters. The specific test process and fracture strength acquisition are as follows:
[0098] 1) Tensile and shear tests of adhesive layer cohesive failure specimens
[0099] First, the tensile test of the butt joint specimen with cohesive failure of the adhesive layer was carried out and repeated 3 times. The test was carried out on an electronic tensile testing machine. The tensile test of the butt joint specimen requires a common tension and shear fixture, such as Fig. 9 As shown in the figure, the upper end of the common tension and shearing fixture is the clamping end clamped with the testing machine, and the lower end of the fixture is the connecting end connected to the specimen. The internal width of the lower end should be slightly larger than the width of the clamping end of the specimen to ensure that there is a certain gap between the clamping end of the tensile fixture and the butt specimen after assembly.
[0100] During the test, the butt joint specimen and the common clamp for tension and shear are assembled by the pin, and the tensile testing machine clamps the upper and lower ends of the common clamp for tension and shear respectively. After the loading starts, the upper clamping end is fixed and the lower clamping end moves according to the set loading rate. The bonding area of the butt joint specimen begins to tear under the action of tension. The coordination of the tensile clamp and the connector pin ensures that the butt joint specimen is always subjected to a force consistent with the tensile direction at the loading end.
[0101] Record the force-displacement data output by the testing machine, use the peak force as the failure load, and record the failure mode and fracture displacement. The test results are expressed as the arithmetic mean of the failure strength of the failure mode specimens of the adhesive itself. The failure strength σ is calculated by dividing the failure load F by the effective bonding area S. The calculation formula is as follows:
[0102]
[0103] The effective bonding area S refers to the actual bonding area after removing the polytetrafluoroethylene film area.
[0104] The average fracture strength of the three groups of test data is taken as the I-mode fracture strength of the adhesive failure in the extended power exponential damage criterion model (i.e., σ GlueI ).
[0105] The shear test specimens with cohesive failure in the adhesive layer are also subjected to tensile shear test for three times, and the test is carried out on an electronic tensile testing machine. The same tensile shear common fixture is required for testing the specimens. The clamping method of the shear specimen and the tensile shear common fixture and the clamping method of the fixture and the testing machine are the same as those of the tensile test of the butt specimens, which will not be repeated here.
[0106] The method of recording test data and processing data is the same as above. The average fracture strength of the three groups of shear specimens tensile shear test data is taken as the type II and type III fracture strength of the adhesive failure in the extended power exponential damage criterion model (i.e. σ GlueII , σ GlueIII ).
[0107] 2) Tensile test of interface failure mode
[0108] First, a tensile test was conducted on a cross tensile specimen with failed interface between base material A and adhesive layer and repeated three times. The test was conducted on an electronic tensile testing machine. In order to load the cross tensile specimen, a cross tensile test fixture was designed. Fig.10 The fixture is a T-shaped structure. The upper end of the fixture is the clamping end connected to the universal tensile testing machine. The two through holes at the lower end should be aligned with the through holes on the cross tensile specimen. The specimen is fixed to the fixture by bolts and nuts.
[0109] During the test, the cross tensile specimen and the cross tensile fixture are assembled by bolts and nuts, and the tensile testing machine clamps the upper and lower ends of the fixture respectively. After the loading starts, the upper clamping end is fixed and the lower clamping end moves according to the set loading rate. The bonding area of the cross tensile specimen begins to tear under the action of tension.
[0110] Record the force-displacement data output by the testing machine, use the peak force as the failure load, and record the failure mode and fracture displacement. The test results are processed according to formula (2) and expressed as the arithmetic mean of the failure strength of the specimens in the failure mode of the effective base material A and the adhesive layer interface.
[0111] The average fracture strength of the three groups of test data is taken as the mode I fracture strength (i.e. σ interAI ).
[0112] The test and data processing methods of the cross tensile specimen with failure at the interface between the base material B and the adhesive layer are as described above and will not be repeated here. Through the test data processing, the I-type fracture strength (i.e., σ interBI ).
[0113] 3) Shear test of interface failure mode
[0114] First, a tensile shear test was carried out on the single lap specimen with failure at the interface between the parent material A and the adhesive layer and repeated three times. The test was carried out on an electronic tensile testing machine. The single lap specimen was clamped on a universal tensile testing machine. During the specimen preparation, the long axis of the specimen was aligned with the axis of the testing machine through a bonding gasket. The test was carried out at the set loading speed, and the bonding area of the single lap specimen began to tear under the action of tension. The force-displacement data output by the testing machine was recorded, and the test results were processed according to formula (2) and expressed as the arithmetic mean of the failure strength of the specimens in the effective parent material A and adhesive layer interface failure mode.
[0115] The average fracture strength of the three groups of test data is taken as the type II and type III fracture strength of the interface failure between the base material A and the adhesive layer in the extended power exponential damage criterion model (i.e., σ interAII , σ interAIII ).
[0116] The test and data processing methods of the single lap joint specimen with failure at the interface between the parent material B and the adhesive layer are as described above and will not be repeated here. Through the test data processing, the type II and type III fracture strengths (i.e., σ interBII , σ interBIII ).
[0117] The fracture strength parameters obtained from the above tests are sorted out and filled into the denominator of the extended power exponential damage criterion model accordingly, thus obtaining the coupled failure extended power exponential damage criterion model with unknown power exponent.
[0118] 4. Power exponent parameter acquisition process
[0119] Step (1): Prepare a sample to obtain power exponential parameters
[0120] 1) Preparation of heterogeneous single lap specimens with variable thickness
[0121] Single lap specimens of variable thickness base material A and constant thickness base material B with three different slopes were prepared. During the preparation, there was no need to insert polytetrafluoroethylene film to create pre-cracks, so that multiple failure mode coupling could occur naturally during the fracture process.
[0122] The sample is prepared by the single lap specimen preparation device mentioned above. During the preparation, a sample with the same slope as the variable thickness sample is placed in advance in the groove of the rear plate or the pressure plate to constrain the sample, and then the variable thickness sample to be glued is placed, so that the two variable thickness samples are fitted together to ensure that the sample bonding surface is horizontal and the bonding thickness is consistent. The rest of the preparation process is consistent with the single lap specimen preparation process of interface failure, and the step of preparing pre-cracks is omitted.
[0123] Step (2): Power exponential parameter acquisition test
[0124] The single lap joint adhesive specimens of three different slopes of base material A and equal thickness base material B were subjected to 30° tension-shear coupling test and 60° tension-shear coupling test respectively. In order to load the specimens with tension-shear coupling, a tension-shear coupling test fixture was designed as follows: Fig.11 As shown. The fixture is an arc-shaped structure. The fixture and the specimen assembly end form angles of 30° and 60° with the axis of the testing machine. The specimen clamping end is assembled with the tension-shear coupling fixture by bolts. The test process is consistent with the above. The experimental data are sorted and the force-displacement curve of each group of tests is obtained. The fracture strength is calculated by formula (2). Based on an extended power exponential damage criterion model of heterogeneous adhesive joints, each of the above experimental conditions is simulated, and the RSME (root mean square error) between the fracture strength value of the simulation result and the fracture strength value of the test result is compared by updating and iterating the power exponent (i.e., α1, β1, α2, β2, α3, β3) to evaluate the error of the simulation fitting (the specific process is the existing technology). If RSME < 0.05, the accuracy requirement is met, and the power exponent of the simulation simulation is the required power exponent parameter; if it cannot be met, another slope of variable thickness base material A and equal thickness base material B single lap adhesive specimens are introduced, and 30° tension-shear coupling tests and 60° tension-shear coupling tests are carried out respectively. The test results are brought into the power exponential iteration of the simulation fitting test curve to determine the power exponent value that meets the accuracy requirement, and so on.
[0125] 5. The fracture strength parameter and power exponent parameter are determined through the above process, and are substituted into formula (1) to be used as the fracture strength model in the constitutive model of the adhesive in the simulation of heterogeneous adhesive joints to determine whether the heterogeneous adhesive joints begin to fail.
[0126] The embodiments are preferred implementations of the present invention, but the present invention is not limited to the above-mentioned implementations. Any obvious improvements, substitutions or modifications that can be made by those skilled in the art without departing from the essential content of the present invention belong to the protection scope of the present invention.
Claims
1. A damage initiation characterization method for coupled failure behavior of heterogeneous adhesive joints, characterized by: (1) Construct an extended power exponential damage criterion model for coupled failure of adhesive joints: Where: interAIC , σ interAIIC , σ interAIIIC are the stress values of type I, type II and type III fracture forms of the interface failure between the adhesive and the base material A, σ interBIC , σ interBIIC , σ interBIIIC are the stress values of type I, type II and type III fracture forms of the interface failure between the adhesive and the base material B, σ GlueIC , σ GlueIIC , σ GlueIIIC are the stress values of type I, type II and type III fracture forms of the adhesive failure, σ interAI , σ interAII , σ interAIII are the strength values of type I, type II and type III fracture modes of the interface failure between the adhesive and the base material A when they exist separately, σ interBI , σ interBII , σ interBIII are the strength values of type I, type II and type III fracture modes of the interface failure between the adhesive and the base material B when they exist separately, σ GlueI , σ GlueII , σ GlueIII are the strength values of type I, type II and type III fracture modes of adhesive failure when they exist alone, respectively; the power exponents α1 and β1 represent the coupling effects of the three different fracture modes on its fracture behavior when the interface between adhesive and base material A fails; the power exponents α2 and β2 represent the coupling effects of the three different fracture modes on its fracture behavior when the interface between adhesive and base material B fails; the power exponents α3 and β3 represent the coupling effects of the three different fracture modes on its fracture behavior when the adhesive fails itself; (2) Prepare butt joint specimens with cohesive failure of the adhesive layer and conduct tensile strength tests. The average fracture strength of the test data is taken as σ GlueI ; Prepare shear specimens with cohesive failure of the adhesive layer, conduct shear strength tests, and use the average fracture strength of the test data as σ GlueII or GlueIII ; A cross tensile specimen with interface failure on the A side of the parent material was prepared and a tensile strength test was carried out. The average fracture strength of the test data was taken as σ interAI ; Prepare single lap joint specimens with interface failure on the parent material A side, conduct shear strength tests, and use the average fracture strength of the test data as σ interAII or interAIII ; A cross tensile specimen with interface failure on the B side of the parent material was prepared and a tensile strength test was performed. The average fracture strength of the test data was taken as σ interBI ; Prepare single lap joint specimens with interface failure on the B side of the parent material, conduct shear strength tests, and use the average fracture strength of the test data as σ interBII or interBIII ; (3) Prepare single lap joint specimens of variable thickness base material A and constant thickness base material B with three different slopes, and conduct 30° tension-shear coupling test and 60° tension-shear coupling test respectively; obtain the force-displacement curve of each group of experiments from the experimental data and calculate the corresponding fracture strength value, simulate each group of experimental conditions, and perform error analysis between the fracture strength value calculated by the simulation result curve and the fracture strength value obtained by the experiment through the update and iteration of the power exponent. When RSME is less than 0.05, the accuracy requirement is met, and the power exponent of the simulation is the power exponent parameter calculated; (4) The determined σ GlueI , σ GlueII , σ GlueIII , σ interAI , σ interAII , σ interAIII , σ interBI , σ interBII , σ interBIII The sum power exponent is substituted into formula (1) and used as the fracture strength model in the constitutive model of the adhesive in the simulation of heterogeneous adhesive joints to determine whether the heterogeneous adhesive joints begin to fail.
2. The damage initiation characterization method for coupling failure behavior of heterogeneous adhesive joints according to claim 1 is characterized in that: The device for preparing a butt joint specimen of adhesive layer cohesive failure comprises a tool 1 front plate (101), a tool 1 rear plate (102), a tool 1 bottom plate (103) and a tool 1 feed screw (104); the tool 1 bottom plate (103) is in a stepped shape, the tool 1 front plate (101) is mounted at the bottom end of the higher step, and the tool 1 rear plate (102) is mounted at the bottom end of the lower step; a groove for placing a specimen is provided on the lower end of the step of the tool 1 bottom plate (103); and the tool 1 feed screw (104) is mounted on the tool 1 front plate (101).
3. The damage initiation characterization method for coupling failure behavior of heterogeneous adhesive joints according to claim 1 is characterized in that: The device for preparing a shearing specimen of cohesive failure of an adhesive layer comprises a front plate (201) of a tool 2, a rear plate (202) of a tool 2, a bottom plate (203) of a tool 2, a pressure plate (204) of a tool 2 and a feed screw (205) of a tool 2; the bottom plate (203) of the tool 2 is in a stepped shape, the bottom of the front plate (201) of the tool 2 is mounted on a higher end of the step, and the bottom of the rear plate (202) of the tool 2 is mounted on a lower end of the step; the pressure plate (204) of the tool 2 is placed between the front plate (201) of the tool 2 and the rear plate (202) of the tool 2 and is located on a lower level of the step; the feed screw (205) of the tool 2 is mounted on the front plate (201) of the tool 2; and a limiting boss is provided in the middle of the bottom plate (203) of the tool 2 for lateral positioning of the shearing specimen.
4. The damage initiation characterization method for coupling failure behavior of heterogeneous adhesive joints according to claim 1 is characterized in that: The device for preparing a cross tensile specimen comprises a tool 3 front plate (301), a tool 3 rear plate (302), a tool 3 connecting plate (303), a tool 3 pressing plate (304) and a tool 3 feeding screw (305); the tool 3 connecting plate (303) is in a "C" shape, and the horizontal surface is in a stepped shape, the lower part of the tool 3 front plate (301) is connected to the higher side of the tool 3 connecting plate (303), and the lower part of the tool 3 rear plate (302) is connected to the lower side of the tool 3 connecting plate (303) The tool 3 pressing plate (304) is in an inverted "convex" shape, placed between the tool 3 front plate (301) and the tool 3 rear plate (302), and located on a lower level of the ladder; the tool 3 feed screw (305) is installed on the tool 3 front plate (301); the tool 3 pressing plate (304) is provided with a groove on a horizontal plane perpendicular to the direction of the feed screw, and the tool 3 rear plate (302) is also provided with a groove on a vertical plane perpendicular to the direction of the feed screw, for placing the sample.
5. The damage initiation characterization method for coupling failure behavior of heterogeneous adhesive joints according to claim 1 is characterized in that: The device for preparing a single lap specimen comprises a front plate (401) of a tooling 4, a rear plate (402) of a tooling 4, a bottom plate (403) of a tooling 4, a pressure plate (404) of a tooling 4 and a feed screw (405) of a tooling 4; the bottom plate (403) of the tooling 4 is in a stepped shape, the bottom of the front plate (401) of the tooling 4 is installed at a higher end of the step, and the bottom of the rear plate (402) of the tooling 4 is installed at a lower end of the step; the pressure plate (404) of the tooling 4 is located between the front plate (401) of the tooling 4 and the rear plate (402) of the tooling 4 and is located on a lower level of the step; the feed screw (405) of the tooling 4 is installed on the front plate (401) of the tooling 4; the pressure plate (404) of the tooling 4 and the rear plate (402) of the tooling 4 are both designed with grooves for placing specimens and gaskets in a horizontal plane perpendicular to the direction of the feed screw, and the grooves on both sides are rotationally symmetrical.
6. The damage initiation characterization method for coupling failure behavior of heterogeneous adhesive joints according to claim 1 is characterized in that: In the above (2), during the preparation of the bonding specimen, cracks are preformed by laying a polytetrafluoroethylene film to guide the crack propagation of the bonding specimen.
7. The damage initiation characterization method for coupling failure behavior of heterogeneous adhesive joints according to claim 6 is characterized in that: In (2), when preparing the sample, it is necessary to apply adhesive on the sample, and select the adhesive layer control gasket according to the thickness of the adhesive layer, wherein: when preparing the butt joint sample with cohesive failure of the adhesive layer, the thickness of the adhesive layer T glue1 Control the thickness of the gasket T with the glue layer shim Satisfaction: T glue1 =T shim -T boss1 -T boss2 , where T boss1 is the height of the butt-jointed specimen boss at one end, T boss2 is the height of the butt specimen boss at the other end; when preparing shear specimens for cohesive failure of the adhesive layer, the adhesive layer thickness T glue2 Control the thickness of the gasket T with the glue layer shim Satisfaction: T glue2 =T Loading +T shim -T Bonding1 -T Bonding2 , where T Loading is the width of the specimen loading end, T Bonding1 T is the width of the bonding end of the shear specimen at one end. Bonding2 is the width of the bonding end of the shear specimen at the other end; when preparing the cross tensile specimen, the thickness of the adhesive layer T glue3 Control the thickness of the gasket T with the glue layer shim Satisfaction: T glue3 =T shim +2*T groove -T sample , where T groove T is the depth of the grooves pre-cut between the pressure plate and the back plate. sample is the thickness of the cross tensile specimen; when preparing single lap specimens, the thickness of the adhesive layer is T glue4 Control the thickness of the gasket T with the glue layer shim Satisfaction: T glue4 =T shim +2*T groove -T' sample , where T groove The depth of the grooves pre-cut on the pressure plate and the back plate, T' sample is the thickness of the single lap specimen.
8. The damage initiation characterization method for coupling failure behavior of heterogeneous adhesive joints according to claim 1 is characterized in that: When the butt joint specimen with cohesive failure of the adhesive layer is subjected to tensile and shear strength tests, the butt joint specimen needs to be equipped with a common tension and shearing fixture. The upper end of the common tension and shearing fixture is a clamping end clamped with a testing machine, and the lower connecting end is provided with a space for placing the specimen. During the test, the butt joint specimen and the common tension and shearing fixture are assembled by a latch.
9. The damage initiation characterization method for coupling failure behavior of heterogeneous adhesive joints according to claim 1 is characterized in that: When the cross tensile specimen with failed interface on the A / B side of the parent material is subjected to tensile strength test, a T-shaped test fixture is provided, the upper end of the fixture is the clamping end connected to the universal tensile testing machine, and the lower end is fixed to the specimen.
10. The damage initiation characterization method for coupling failure behavior of heterogeneous adhesive joints according to claim 1 is characterized in that: When the single lap specimen is subjected to the tension-shear coupling test, an arc-shaped fixture is provided. The fixture and the specimen assembly end form an angle of 30° and 60° with the axis of the testing machine, and the specimen clamping end is assembled with the fixture.
Citation Information
Patent Citations
Creep-fatigue-oxidation real-time damage accumulation evaluation method for material
CN111879636A
Method and system for evaluating structural strength of damaged cementing repair of resin-based composite material
CN115481550A
Interlayer eccentric structure joint R angle failure mode control method