A magnetic composite corrosion-resistant microwave absorbing material and its application
By preparing an ultrathin heterogeneous capsule structure with an inorganic inner shell and an organosilicon polymer outer shell on the surface of magnetic micropowder, the problems of insufficient corrosion resistance and microwave absorption performance of existing core-shell structure materials in extreme environments are solved, achieving efficient equipment protection and performance improvement.
Patent Information
- Application Number
- CN202311017696.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-14
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-08-14
AI Technical Summary
Existing core-shell structure materials are complex and costly to prepare, increasing material thickness and weight, and may reduce microwave absorption performance, making them unable to effectively protect 5G devices in extreme environments.
By employing an ultrathin organic/inorganic heterocapsule structure, an inorganic inner shell and an organic silicon polymer outer shell are prepared on the surface of magnetic micropowder, simplifying the process and enhancing corrosion resistance and microwave absorption performance.
It achieves effective protection for 5G equipment in extreme environments, possesses excellent corrosion resistance and microwave absorption performance, and has a simple process and low cost.
Smart Images

Figure CN117062423B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of microwave absorbing materials technology, specifically to a magnetic composite corrosion-resistant microwave absorbing material and its application. Background Technology
[0002] Currently, 5G communication technology, using gigahertz electromagnetic waves as a medium, enables mobile and industrial equipment to achieve ultra-high information transmission efficiency, triggering exciting upgrades in the intelligent automation control and communication industries. However, the electromagnetic radiation derived from high-frequency electromagnetic waves can cause electromagnetic interference to sensitive equipment and have potential impacts on human health. Absorbing materials, which can attenuate electromagnetic waves and convert them into heat energy, have become a focus of attention in addressing electromagnetic radiation. However, as 5G devices expand into industrial IoT and marine military applications, the complex and extreme environments of the ocean, acid rain, and alkaline chemicals inevitably cause widespread corrosion of ferromagnetic absorbing materials (such as carbonyl iron, FeSiAl, and FeCo), ultimately leading to the failure of the shielding protection function of 5G devices. Therefore, multifunctional materials that can self-regulate against external stimuli are crucial, with bifunctional materials combining excellent corrosion resistance and broadband absorption performance being a key research focus.
[0003] The mainstream approach to preparing bifunctional materials with corrosion resistance and good microwave absorption properties is to construct one or more core-shell structures on the substrate surface using heterogeneous interface engineering. The advantages of this core-shell structure include: First, it can inherit the unique magnetic, dielectric, and other electromagnetic properties of the original material, maximizing impedance matching and enhancing energy dissipation probability. Second, the heterogeneous interface formed between the core-shell structure and the substrate introduces a series of remarkable physicochemical properties, such as band alignment, space charge, electron transport, lattice defects, lattice strain, and pinning effects. These properties significantly influence dipole polarization, dielectric loss, and magnetic response, thereby affecting microwave absorption performance. Third, the core-shell structure is generally composed of inert materials, forming a physical barrier on the substrate surface that prevents corrosive media from eroding the substrate. Among these, selecting the correct fabrication process, chemical composition, and optimizing the interface structure design are crucial for regulating the electromagnetic properties and corrosion resistance of the substrate.
[0004] To enhance the corrosion resistance of FeSiAl in extremely humid and salt spray environments, W Tian et al. prepared a FeSiAl@ZnO@Al2O3 core-shell structure using ZnO@Al2O3 as a barrier. The FeSiAl@ZnO@Al2O3 exhibited a minimum reflection loss (RLmin) of -50.6 dB and an effective bandwidth (EAB) of 1.5 GHz at 3.4 GHz. Compared to pure FeSiAl magnetic micropowder (RLmin -13.5 dB, EAB 0.5 GHz), the absolute value of the minimum reflection loss (RLmin) and the effective bandwidth of FeSiAl@ZnO@Al2O3 were increased by approximately 3.7 times and 3 times, respectively. Furthermore, the multi-level barrier effect of the ZnO@Al2O3 inert ceramic layer improved the corrosion resistance of FeSiAl by 9.0 times. W Tian et al. synthesized a fluorine-free core-shell carbonyl iron-organosilicon absorber, CI@SiO2 / HMDS, using tetraethyl orthosilicate (TEOS) and hexamethyldisilazane (HMDS) as precursors. The CI@SiO2 / HMDS composite material achieved a maximum radar cross section (RCS) reduction of approximately 16.5 dB·m at a detection θ of 0°. 2 CI@SiO2 / HMDS has a contact angle of 132.5°, demonstrating good shielding ability against corrosive media. However, after coating the CI surface with SiO2 / HDMS, the microwave absorption performance of CI was not significantly enhanced.
[0005] Therefore, while the construction of core-shell structures can enhance the corrosion resistance and microwave absorption properties of the substrate, it presents the following problems: First, although the core-shell layer prepared by atomic deposition technology enhances the corrosion resistance and microwave absorption properties of the substrate to a certain extent, its process is relatively complex and costly, limiting its widespread application. Second, adding a core-shell layer increases the thickness and weight of the material, which may limit certain applications. Third, the construction of the core-shell layer may lead to problems such as magnetic moment confinement and local magnetic field inhomogeneity, thereby reducing the ferromagnetic properties of the material; the microwave scattering, reflection, or interference phenomena introduced by the core-shell layer are insufficient to compensate for the loss of ferromagnetic properties, thus leading to a decrease in microwave absorption performance.
[0006] Therefore, it is of great significance to develop an ultrathin core-shell structure with synergistic enhancement of corrosion resistance and microwave performance based on appropriate chemical composition and simple, refined control strategies. Summary of the Invention
[0007] To overcome the above defects, the preparation method of the ultrathin organic / inorganic heterocapsule of the present invention solves the problem of easy corrosion of electromagnetic radiation absorbing gold materials, and obtains ultrathin organic / inorganic heterocapsules with excellent corrosion resistance and enhanced microwave absorption performance.
[0008] A magnetic composite corrosion-resistant microwave absorbing material is disclosed, wherein the magnetic composite corrosion-resistant microwave absorbing material has a heterogeneous core-shell structure, the core being magnetic micropowder, and the shell being an inorganic / organic heterogeneous shell; the inorganic / organic heterogeneous shell comprises an inorganic inner shell and an organic silicon polymer outer shell, the inorganic inner shell being attached to the surface of the magnetic micropowder, and the organic silicon polymer outer shell being attached to the surface of the inorganic inner shell, the chemical structural formula of the organic silicon polymer being as follows:
[0009]
[0010] Wherein, R1 represents methyl, ethyl or -CH2CH2CnF 2n+1 R2 represents methyl, ethyl, or -CH2CH2C n F 2n+1 , where n represents a natural number from 2 to 10.
[0011] In one specific embodiment of the present invention, the inorganic inner shell is any one of SiO2, ZnO, Al2O3, and TiO2.
[0012] In one specific embodiment of the present invention, the inorganic inner shell is SiO2; the method for preparing the SiO2 on the surface of magnetic micro powder includes the following steps:
[0013] A dispersion of magnetic micropowder, ammonia, and orthosilicate were mixed and hydrolyzed to prepare SiO2 on the surface of the magnetic micropowder; wherein the volume ratio of the dispersion, ammonia, and orthosilicate was (310-420):(1-5):(0.5-3).
[0014] In one specific embodiment of the present invention, the mass-volume concentration of magnetic micropowder in the magnetic micropowder dispersion is 23.8–32.2 mg / mL; the dispersant of the magnetic micropowder dispersion is a 75–85 vol% ethanol aqueous solution or a 75–85 vol% methanol aqueous solution.
[0015] In one specific embodiment of the present invention, the hydrolysis reaction takes 0.5 to 2 hours and the hydrolysis reaction takes 30 to 60°C.
[0016] In one specific embodiment of the present invention, the method for preparing the organosilicon polymer includes the following reaction equation:
[0017]
[0018] Wherein, R1 represents methyl, ethyl or -CH2CH2C n F 2n+1 R2 represents methyl, ethyl, or -CH2CH2C n F 2n+1, n represents a natural number from 2 to 10; R3 represents methyl, ethyl or propyl;
[0019] The specific reaction steps are as follows:
[0020] Compound a, compound b, surfactant, stabilizer and catalyst are mixed and polymerized to obtain organosilicon polymer; wherein the mass ratio of compound a, compound b, surfactant, stabilizer and catalyst is (1~100):(1~100):(0.1~1):(0.5~1.5):(0.1~0.5).
[0021] In this invention, when R1 and R2 are the same, compound a and compound b are the same. Even if compound a and compound b are the same, a polymerization reaction as shown in the reaction equation can still occur. The mechanism of the polymerization reaction is as follows: the methoxy or ethoxy groups of the molecules of compound a and compound b break down to generate hydroxyl groups and methanol or ethanol. The hydroxyl groups between adjacent molecules undergo dehydration bonding to obtain an organosilicon polymer. The R1 and R2 functional groups in the organosilicon polymer do not participate in the bonding reaction. Therefore, when the polymer forms an organic shell from an inorganic inner shell, it provides dipole polarization, enriches the interface of the organic shell, increases the interface polarization mechanism, and also provides wave transmission and optimizes impedance matching.
[0022] In this invention, the surfactant can enhance the surface activity of the inorganic inner shell, thereby promoting the adhesion of the organosilicon polymer obtained from the polymerization reaction to the surface of the inorganic inner shell to form an organic polymer outer shell; the stabilizer can react with free radicals or ions to inhibit their generation and reaction, thereby improving the stability and efficiency of the reaction. By adjusting the rate and direction of the polymerization reaction, the desired polymer structure and properties can be obtained.
[0023] In one specific embodiment of the present invention, the surfactant is selected from any one or more of methylbenzenesulfonic acid, ethylbenzenesulfonic acid, and propylbenzenesulfonic acid; the stabilizer is polyethylene glycol, and the degree of polymerization of the polyethylene glycol is 200 to 8000; the catalyst is any one or more of dimethylamide, diethylamide, and dipropylamide.
[0024] In one specific embodiment of the present invention, the polymerization reaction takes 0.5 to 2 hours and the polymerization reaction temperature is 40 to 70°C.
[0025] In one specific embodiment of the present invention, the magnetic micro powder is any one of carbonyl iron, FeNi, FeCo, and FeSiAl; the particle size of the magnetic micro powder is 10-74 μm; and the thickness of the inorganic / organic heteroshell is 20-50 nm.
[0026] The aforementioned magnetic composite corrosion-resistant absorbing material is used for microwave absorption.
[0027] The preparation method of the above-mentioned magnetic composite corrosion-resistant microwave absorbing material includes the following steps:
[0028] 1) Preparation of inner shell: Mix the suspension of magnetic micro powder with the reaction solution of inorganic inner shell, and attach the inorganic inner shell to the surface of magnetic micro powder to obtain a mixed suspension;
[0029] 2) Preparation of the outer shell: The mixed suspension is mixed with the reaction liquid of the organic shell, and the organic shell is attached to the surface of the inorganic inner shell to obtain a magnetic composite corrosion-resistant microwave absorbing material.
[0030] The preparation method of this invention involves a primary and secondary reaction, using magnetic metal micropowder as the core, to obtain a shell with a thickness of 20-50 nm on the surface of the magnetic metal micropowder, ultimately producing an ultrathin organic / inorganic heterocapsule. The shell of this ultrathin organic / inorganic heterocapsule is stably attached to the surface of the metal micropowder core, giving it excellent corrosion resistance and microwave absorption performance. The process of this invention is simple, low-cost, and has a high yield, making it suitable for industrial production. Attached Figure Description
[0031] Figure 1 This is a SEM image of FeNi@SiO2@F13 / MTMS-1 obtained in Example 1 of the present invention;
[0032] Figure 2 This is a SEM image of the FeNi magnetic metal micropowder from Example 1 of the present invention;
[0033] Figure 3 This is a SEM image of FeNi@SiO2 obtained in Example 1 of the present invention;
[0034] Figure 4 This is a SEM image of FeNi@SiO2@F13 / MTMS-2 obtained in Example 2 of the present invention;
[0035] Figure 5 This is a SEM image of FeNi@SiO2@F13 / MTMS-3 obtained in Example 3 of the present invention;
[0036] Figure 6 The XPS graphs obtained from XPS testing in Embodiments 1-3 of this invention are shown.
[0037] Figure 7 The TEM image is obtained by TEM testing of FeNi@SiO2@F13 / MTMS-1 in Example 1 of the present invention;
[0038] Figure 8 The TEM image obtained by TEM testing of FeNi@SiO2@F13 / MTMS-2 in Example 2 of the present invention;
[0039] Figure 9 The TEM image obtained by TEM testing of FeNi@SiO2@F13 / MTMS-3 in Example 3 of the present invention;
[0040] Figure 10 The graphs shown are RL curves obtained from RL testing in Embodiments 1-3 of this invention.
[0041] Figure 11 The images shown are Tafel curves obtained from the Tafel polarization method in Embodiments 1-3 of this invention. Detailed Implementation
[0042] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be described in detail below. Obviously, the described embodiments are merely some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other implementation methods obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0043] A magnetic composite corrosion-resistant microwave absorbing material is disclosed, wherein the magnetic composite corrosion-resistant microwave absorbing material has a heterogeneous core-shell structure, the core being magnetic micropowder, and the shell being an inorganic / organic heterogeneous shell; the inorganic / organic heterogeneous shell comprises an inorganic inner shell and an organic silicon polymer outer shell, the inorganic inner shell being attached to the surface of the magnetic micropowder, and the organic silicon polymer outer shell being attached to the surface of the inorganic inner shell, the chemical structural formula of the organic silicon polymer being as follows:
[0044]
[0045] Wherein, R1 represents methyl, ethyl or -CH2CH2C n F 2n+1 R2 represents methyl, ethyl, or -CH2CH2C n F 2n+1 , where n represents a natural number from 2 to 10.
[0046] In some instances, the inorganic inner shell is any one of SiO2, ZnO, Al2O3, and TiO2.
[0047] In some instances, the inorganic inner shell is SiO2; the method for preparing SiO2 on the surface of magnetic micropowder includes the following steps: mixing a dispersion of magnetic micropowder, ammonia and orthosilicate, hydrolyzing the mixture, and preparing SiO2 on the surface of magnetic micropowder; wherein the volume ratio of the dispersion, ammonia and orthosilicate is (310-420):(1-5):(0.5-3).
[0048] In some instances, ammonia is 5m ammonia water; orthosilicate is tetraethyl orthosilicate, analytical grade.
[0049] In this invention, to avoid the precipitation of SiO2 crystals generated by the hydrolysis reaction, magnetic micropowder is mixed with ammonia and orthosilicate. The SiO2 generated by the hydrolysis reaction is deposited on the surface of the magnetic micropowder, thereby forming an inorganic inner shell of SiO2.
[0050] In some instances, the mass-volume concentration of magnetic micropowder in the magnetic micropowder dispersion is 23.8–32.2 mg / mL; the dispersant in the magnetic micropowder dispersion is a 75–85 vol% aqueous ethanol solution or a 75–85 vol% aqueous methanol solution.
[0051] In some instances, the hydrolysis reaction takes 0.5 to 2 hours and is carried out at a temperature of 30 to 60°C.
[0052] In some examples, the preparation method of the organosilicon polymer includes the following reaction equations:
[0053]
[0054] Wherein, R1 represents methyl, ethyl or -CH2CH2C n F 2n+1 R2 represents methyl, ethyl, or -CH2CH2C n F 2n+1 , n represents a natural number from 6 to 10; R3 represents methyl, ethyl or propyl;
[0055] The specific reaction steps are as follows:
[0056] Compound a, compound b, surfactant, stabilizer and catalyst are mixed and polymerized to obtain organosilicon polymer; wherein the mass ratio of compound a, compound b, surfactant, stabilizer and catalyst is (1~100):(1~100):(0.1~1):(0.5~1.5):(0.1~0.5).
[0057] In this invention, in order to directly attach the polymer obtained by polymerization to the surface of the inorganic inner shell, the suspension in which SiO2 is deposited on the surface of magnetic micropowder through hydrolysis can be directly mixed with compound a, compound b, surfactant, stabilizer and catalyst, and polymerized, so that the polymer obtained by polymerization directly attaches to the surface of the inorganic inner shell.
[0058] In some instances, when R1 is selected as -CH2CH2C n F 2n+1 When n = 2 and R3 is chosen as ethyl, the name of compound a is 1H,1H,2H,2H-perfluorobutyltriethoxysilane; when R1 is chosen as -CH2CH2C n F2n+1 When n = 10 and R3 is chosen as ethyl, the name of compound a is 1H,1H,2H,2H-perfluorododecyltriethoxysilane; compound a is preferably 1H,1H,2H,2H-perfluorobutyltriethoxysilane, 1H,1H,2H,2H-perfluorooctyltriethoxysilane, or 1H,1H,2H,2H-perfluorododecyltriethoxysilane; experimental studies have found that 1H,1H,2H,2H-perfluorooctyltriethoxysilane or 1H,1H,2H,2H-perfluorododecyltriethoxysilane are more toxic than 1H,1H,2H,2H-perfluorooctyltriethoxysilane. Therefore, compound a is most preferably 1H,1H,2H,2H-perfluorooctyltriethoxysilane, and it was used as a monomer for preparing organosilicon polymer shells in experiments;
[0059] When R2 is chosen as methyl and R3 is chosen as methyl, the name of compound b is methyltrimethoxysilane; when R2 is chosen as ethyl and R3 is chosen as methyl, the name of compound b is ethyltrimethoxysilane; compound b is preferably methyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane or methyltripropoxysilane.
[0060] In some examples, the surfactant is selected from any one or more of methylbenzenesulfonic acid, ethylbenzenesulfonic acid, and propylbenzenesulfonic acid; the stabilizer is polyethylene glycol, and the degree of polymerization of the polyethylene glycol is 200 to 8000; the catalyst is any one or more of dimethylamide, diethylamide, and dipropylamide.
[0061] In some instances, the polymerization reaction takes 0.5 to 2 hours and is carried out at a temperature of 40 to 70°C.
[0062] In some examples, the magnetic micropowder is any one of carbonyl iron, FeNi, FeCo, and FeSiAl; the particle size of the magnetic micropowder is 10–74 μm; and the thickness of the inorganic / organic heteroshell is 20–50 nm.
[0063] The aforementioned magnetic composite corrosion-resistant absorbing material is used for microwave absorption.
[0064] The preparation method of the above-mentioned magnetic composite corrosion-resistant microwave absorbing material includes the following steps:
[0065] 1) Preparation of inner shell: Mix the suspension of magnetic micro powder with the reaction solution of inorganic inner shell, and attach the inorganic inner shell to the surface of magnetic micro powder to obtain a mixed suspension;
[0066] 2) Preparation of the outer shell: The mixed suspension is mixed with the reaction solution of the organic outer shell, and the organic outer shell is attached to the surface of the inorganic inner shell to obtain a magnetic composite corrosion-resistant microwave absorbing material. A magnetic composite corrosion-resistant microwave absorbing material, wherein the magnetic composite corrosion-resistant microwave absorbing material has a heterogeneous core-shell structure, the core is magnetic micropowder, and the shell is an inorganic / organic heterogeneous shell.
[0067] In this invention, a suspension of magnetic micropowder can be mixed with the reaction liquid raw material of an inorganic inner shell. During the reaction process of the reaction liquid itself, the product directly adheres to the surface of the magnetic micropowder, thereby obtaining magnetic micropowder coated with an inorganic inner shell. Similarly, a mixed suspension of magnetic micropowder coated with an inorganic inner shell is mixed with the reaction liquid raw material of an organosilicon polymer. During the polymerization reaction, the organosilicon polymer adheres to the surface of the inorganic inner shell to form an organosilicon polymer outer shell.
[0068] Taking the preparation of a magnetic composite corrosion-resistant microwave absorbing material with a core of FeNi, an inorganic inner shell of SiO2, and an organosilicon polymer outer shell as an example, one of its preparation methods is as follows:
[0069] Mix 310-420 mL of magnetic micro powder in ethanol and water with 1-5 mL of 5 mL ammonia water and 0.5-3 mL of tetraethyl orthosilicate, and hydrolyze at 30-60 °C to obtain a mixed suspension of magnetic micro powder with SiO2 attached.
[0070] The above mixed suspension was mixed with 1-100g of 1H,1H,2H,2H-perfluorooctyltriethoxysilane, 1-100g of dodecylbenzenesulfonic acid, 0.1-1g of dodecylbenzenesulfonic acid, 0.5-1.5g of polyethylene glycol and 0.1-0.5g of dimethylamide, and polymerized at 40-70℃ for 0.5-2h to obtain a magnetic composite corrosion-resistant microwave absorbing material with FeNi as the core, SiO2 as the inorganic inner shell and an organosilicon polymer as the organic outer shell.
[0071] Example 1
[0072] This embodiment provides a magnetic composite corrosion-resistant microwave absorbing material with a heterogeneous core-shell structure. The core is magnetic micropowder, and the shell is an inorganic / organic heterogeneous shell. The inorganic inner shell of the inorganic / organic heterogeneous shell is SiO2, and the organic outer shell is a polymer formed by the polymerization of 1H,1H,2H,2H-perfluorooctyltriethoxysilane (F13) and methyltrimethoxysilane (MTMS).
[0073] The preparation of this magnetic composite corrosion-resistant microwave absorbing material includes the following steps:
[0074] 1) Slowly pour 280 mL of anhydrous ethanol into 70 mL of deionized water and stir for 10 min to obtain an ethanol-water solution.
[0075] 2) Slowly pour 10g of FeNi magnetic micro powder into an ethanol aqueous solution and stir continuously for 10min to obtain a dispersion. Then, add 5m of ammonia water and 2.5mL of tetraethyl orthosilicate to the dispersion in sequence, and hydrolyze at 30℃ for 1h. The SiO2 obtained from the hydrolysis reaction adheres to the surface of the magnetic micro powder to obtain a mixed suspension, labeled as FeNi@SiO2. When detection is required, the mixed suspension is cleaned with deionized water and ethanol and then filtered. The filter residue is vacuum dried to obtain FeNi@SiO2 micro powder for detection.
[0076] 3) Add 0.5 g of dodecylbenzenesulfonic acid, 1 g of polyethylene glycol, 0.2 g of dimethylamide, 2.5 mL of 1H,1H,2H,2H-perfluorooctyltriethoxysilane and 5.5 mL of methyltrimethoxysilane to the mixed suspension, and react at 50 °C for 1 h; wash the final product with a mixture of deionized water and ethanol, filter, and dry the filter residue under vacuum, labeling it as FeNi@SiO2@F13 / MTMS-1.
[0077] The SEM image of FeNi@SiO2@F13 / MTMS-1 obtained in this embodiment is as follows: Figure 1 As shown; the SEM image of the FeNi magnetic metal micro powder in this embodiment is as follows. Figure 2 As shown; the SEM image of FeNi@SiO2 in this embodiment is as follows. Figure 3 As shown; by Figure 2 As can be seen, the surface of FeNi magnetic metal micropowder exhibits a granular surface with a network structure similar to a soccer ball; from Figure 3 It is evident that after coating the surface of FeNi magnetic metal micropowder with a SiO2 layer, there was no significant change in the surface; Figure 1 As can be seen, after 1H,1H,2H,2H-perfluorooctyltriethoxysilane (F13) and methyltrimethoxysilane (MTMS) polymerize and deposit on the FeNi@SiO2 surface, a large number of fine white particles appear on the surface.
[0078] Example 2
[0079] This embodiment provides a magnetic composite corrosion-resistant microwave absorbing material with a heterogeneous core-shell structure. The core is magnetic micropowder, and the shell is an inorganic / organic heterogeneous shell. The inorganic inner shell of the inorganic / organic heterogeneous shell is SiO2, and the organic silicon polymer outer shell is polymerized from 1H,1H,2H,2H-perfluorooctyltriethoxysilane (F13) and methyltrimethoxysilane (MTMS).
[0080] The difference between the preparation of the magnetic composite corrosion-resistant microwave absorbing material in this embodiment and that in Example 1 is that the amount of methyltrimethoxysilane added is 6 mL; the final product obtained after the reaction is labeled as FeNi@SiO2@F13 / MTMS-2.
[0081] The SEM image of FeNi@SiO2@F13 / MTMS-2 obtained in this embodiment is as follows: Figure 4 As shown; by Figure 4 As can be seen, after 1H,1H,2H,2H-perfluorooctyltriethoxysilane (F13) and methyltrimethoxysilane (MTMS) polymerize and deposit on the FeNi@SiO2 surface, a number of fine white particles also appear on the surface.
[0082] Example 3
[0083] This embodiment provides a magnetic composite corrosion-resistant microwave absorbing material with a heterogeneous core-shell structure. The core is magnetic micropowder, and the shell is an inorganic / organic heterogeneous shell. The inorganic inner shell of the inorganic / organic heterogeneous shell is SiO2, and the organic silicon polymer outer shell is polymerized from 1H,1H,2H,2H-perfluorooctyltriethoxysilane (F13) and methyltrimethoxysilane (MTMS).
[0084] The difference between this embodiment and Example 1 is that the amount of methyltrimethoxysilane added is 5 mL.
[0085] The final product obtained after the reaction is labeled FeNi@SiO2@F13 / MTMS-3.
[0086] The SEM image of FeNi@SiO2@F13 / MTMS-3 obtained in this embodiment is as follows: Figure 5 As shown; by Figure 5 As can be seen, after 1H,1H,2H,2H-perfluorooctyltriethoxysilane (F13) and methyltrimethoxysilane (MTMS) polymerize and deposit on the FeNi@SiO2 surface, a number of fine white particles also appear on the surface.
[0087] Performance testing
[0088] XPS testing: XPS testing was performed on FeNi@SiO2@F13 / MTMS from Examples 1-3 based on X-ray photoelectron spectroscopy. The test results are as follows: Figure 6 As shown; by Figure 6 It can be seen that the main chemical elements of FeNi@SiO2@F13 / MTMS-1, FeNi@SiO2@F13 / MTMS-2 and FeNi@SiO2@F13 / MTMS-3 all include Fe, Ni, Si, O, C, N and F.
[0089] TEM testing: The FeNi@SiO2@F13 / MTMS samples from Examples 1-3 were subjected to TEM testing using a transmission electron microscope. The test results are as follows: Figure 7-9 As shown; by Figure 7It can be seen that the thickness of the SiO2@F13 / MTMS heterocapsule shell in FeNi@SiO2@F13 / MTMS-1 is approximately 28 nm; Figure 8 It can be seen that the thickness of the SiO2@F13 / MTMS heterocapsule shell in FeNi@SiO2@F13 / MTMS-2 is approximately 30 nm; Figure 9 It can be seen that the thickness of the SiO2@F13 / MTMS heterocapsule shell in FeNi@SiO2@F13 / MTMS-3 is approximately 27 nm.
[0090] RL testing: RL tests were performed on the FeNi magnetic metal micropowder of Example 1, FeNi@SiO2, FeNi@SiO2@F13 / MTMS-1, FeNi@SiO2@F13 / MTMS-2 of Example 2, and FeNi@SiO2@F13 / MTMS-3 of Example 3. The test results are as follows: Figure 10 As shown; by Figure 10 As can be seen, when the matching degree is 2.0 mm, the effective absorption bandwidth of FeNi magnetic metal micropowder is 5.18 GHz, and the minimum reflection loss is -14.91 dB; the effective absorption bandwidth of FeNi@SiO2 is 7.91 GHz, and the minimum reflection loss is -17.25 dB; the effective absorption bandwidth of FeNi@SiO2@F13 / MTMS-1 is 8.16 GHz, and the minimum reflection loss is -24.03 dB; the effective absorption bandwidth of FeNi@SiO2@F13 / MTMS-2 is 8.01 GHz. The minimum reflection loss is -23.52dB; the effective absorption bandwidth of FeNi@SiO2@F13 / MTMS-3 is 8.10GHz, and the minimum reflection loss is -23.45dB. Compared with FeNi magnetic metal micropowder, FeNi@SiO2, FeNi@SiO2@F13 / MTMS-2, and FeNi@SiO2@F13 / MTMS-3, FeNi@SiO2@F13 / MTMS-1 has a wider effective absorption bandwidth and the lowest reflection loss, exhibiting the best microwave absorption performance.
[0091] Tafel polarization test: Tafel tests were performed on the FeNi magnetic micropowder of Example 1, FeNi@SiO2, FeNi@SiO2@F13 / MTMS-1, FeNi@SiO2@F13 / MTMS-2 of Example 2, and FeNi@SiO2@F13 / MTMS-3 of Example 3. The test results are as follows: Figure 11 As shown; by Figure 11It can be seen that the corrosion potential of FeNi magnetic micro powder is -0.622V, the corrosion potential of FeNi@SiO2 is -0.308V, the corrosion potential of FeNi@SiO2@F13 / MTMS-1 is -0.007V, the corrosion potential of FeNi@SiO2@F13 / MTMS-2 is -0.017V, and the corrosion potential of FeNi@SiO2@F13 / MTMS-3 is -0.012V. Compared with FeNi magnetic metal micro powder, FeNi@SiO2, FeNi@SiO2@F13 / MTMS-2, and FeNi@SiO2@F13 / MTMS-3, FeNi@SiO2@F13 / MTMS-1 has a higher corrosion potential and exhibits the best salt corrosion resistance.
[0092] Existing magnetic composite corrosion-resistant microwave absorbing materials, such as FeSiAl@ZnO@Al2O3 prepared in reference 1, "Atomic-Scale Layer-by-Layer Deposition of FeSiAl@ZnO@Al2O3 Hybrid with Threshold Anti-Corrosion and Ultra-High Microwave Absorption Properties in Low-Frequency Bands" (W. Tian, et al, Nano-Micro Letters 13(1)(2021)161.), have a corrosion current density of 8196 nA·cm. 2 Its corrosion resistance is poor, and its corrosion current density is lower than that of FeNi@SiO2@F13 / MTMS-2 in Example 2 of this invention, which has a corrosion current density of 5.59 nA·cm. 2 For example, in reference 2, "Large-scale synthesis of fluorine-freecarbonyl iron-organic silicon hydrophobic absorbers with long-term corrosion protection property" (Tian W, et al. Nano Research, 2022, 15(10): 9479-9491.), CI@SiO2 / HMDS was prepared with a corrosion current density of 653 nA·cm. 2 Its corrosion resistance is still relatively poor, and its corrosion current density is lower than that of FeNi@SiO2@F13 / MTMS-2 in Example 2 of this invention, which has a corrosion current density of 5.59 nA·cm. 2 .
[0093] Compared with existing magnetic composite corrosion-resistant absorbing materials, the magnetic composite corrosion-resistant absorbing material of the present invention not only has better corrosion resistance, but also enhances the wave absorption effect.
Claims
1. A magnetic composite corrosion-resistant wave-absorbing material, characterized in that, The magnetic composite corrosion-resistant microwave absorbing material has a heterogeneous core-shell structure. The core is magnetic micropowder, and the shell is an inorganic / organic heterogeneous shell. The inorganic / organic heterogeneous shell includes an inorganic inner shell and an organic silicon polymer outer shell. The inorganic inner shell is attached to the surface of the magnetic micropowder, and the organic silicon polymer outer shell is attached to the surface of the inorganic inner shell. The chemical structural formula of the organic silicon polymer is as follows: wherein R1 represents a methyl group, an ethyl group or -CH2CH2C n F 2n+1 , R2 represents a methyl group, an ethyl group or -CH2CH2C n F 2n+1 , and n represents a natural number of 2 to 10. The preparation method of the organosilicon polymer includes the following reaction equation: Wherein, R1 represents methyl, ethyl or -CH2CH2CnF 2n+1 R2 represents methyl, ethyl, or -CH2CH2CnF 2n+1 , n represents a natural number from 2 to 10; R3 represents methyl, ethyl or propyl; The specific reaction steps are as follows: Compound a, compound b, surfactant, stabilizer and catalyst are mixed and polymerized to obtain organosilicon polymer; wherein the mass ratio of compound a, compound b, surfactant, stabilizer and catalyst is (1~100):(1~100):(0.1~1):(0.5~1.5):(0.1~0.5).
2. The magnetic composite corrosion-resistant wave-absorbing material according to claim 1, characterized in that, The inorganic inner shell is any one of SiO2, ZnO, Al2O3, and TiO2.
3. The magnetic composite corrosion-resistant wave-absorbing material according to claim 2, characterized in that, The inorganic inner shell is SiO2; the method for preparing the SiO2 on the surface of magnetic micro powder includes the following steps: A dispersion of magnetic micropowder, ammonia, and orthosilicate were mixed and hydrolyzed to prepare SiO2 on the surface of the magnetic micropowder; wherein the volume ratio of the dispersion, ammonia, and orthosilicate was (310-420):(1-5):(0.5-3).
4. The magnetic composite corrosion-resistant wave-absorbing material according to claim 3, characterized in that, The magnetic micropowder dispersion has a mass-volume concentration of 23.8–32.2 mg / mL; the dispersant in the magnetic micropowder dispersion is a 75–85 vol% ethanol aqueous solution or a 75–85 vol% methanol aqueous solution.
5. The magnetic composite corrosion-resistant wave-absorbing material according to claim 3, characterized in that, The hydrolysis reaction takes 0.5 to 2 hours and is carried out at a temperature of 30 to 60°C.
6. The magnetic composite corrosion-resistant wave-absorbing material according to claim 1, characterized in that, The surfactant is selected from any one or more of methylbenzenesulfonic acid, ethylbenzenesulfonic acid, and propylbenzenesulfonic acid; the stabilizer is polyethylene glycol, and the degree of polymerization of the polyethylene glycol is 200 to 8000; the catalyst is any one or more of dimethylamide, diethylamide, and dipropylamide.
7. The magnetic composite corrosion-resistant wave-absorbing material according to claim 1, characterized in that, The polymerization reaction takes 0.5 to 2 hours and is carried out at a temperature of 40 to 70°C.
8. The magnetic composite corrosion-resistant wave-absorbing material according to claim 1, characterized in that, The magnetic micro powder is any one of carbonyl iron, FeNi, FeCo, and FeSiAl; the particle size of the magnetic micro powder is 10–74 μm; and the thickness of the inorganic / organic heteroshell is 20–50 nm.
9. The use of the magnetic composite corrosion-resistant absorbing material according to any one of claims 1-8 for microwave absorption.
Citation Information
Patent Citations
Preparation method of corrosion-resistant wave-absorbing coating containing core-shell structure type magnetic absorbent
CN111001549A
Preparation method of FeSiAl-based organic-inorganic double-layer core-shell structure
CN113402920A
Cited By
Corrosion-resistant pure magnetic porous foam wave-absorbing material and preparation method thereof
CN119603946A