Preparation method of centimeter-scale ultra-tough, ultra-conductive and ultra-hard carbon composite material
A novel method for preparing centimeter-scale carbon composites addresses the limitations of small sample sizes and synthesis conditions, resulting in materials with superior conductivity and hardness for practical use.
Patent Information
- Application Number
- CN202310915672.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-07-20
AI Technical Summary
Existing carbon composites, such as diamond-graphite nanocomposites, are limited by small sample sizes and harsh synthesis conditions, preventing the realization of centimeter-scale materials with both high conductivity and hardness, which are necessary for practical applications.
A method involving pre-treatment of nanodiamonds, assembly in a high-pressure assembly block, and subsequent high-temperature, high-pressure treatment to form a centimeter-scale carbon composite material with a mixed sp² and sp³ phase structure, using a zirconium/molybdenum cup and graphite mold.
The method produces a carbon composite material with enhanced conductivity and hardness, achieving a Vickers hardness of 55.8 GPa and conductivity of 2×10⁴ S m⁻¹ at room temperature, with fracture toughness up to 19.8 MPa m⁻¹⁄₂, suitable for industrial applications.
Smart Images

Figure CN117088366B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of novel carbon composite materials, and in particular to a method for preparing centimeter-level ultra-tough, ultra-conductive and ultra-hard carbon composite materials. Background Art
[0002] Diamond has the advantages of extremely high hardness, unparalleled high thermal conductivity and excellent chemical inertness, and is a widely used material. Although diamond is the hardest natural material, its toughness and conductivity are poor. At present, it can be toughened by introducing structural structures such as nanotwins, but diamond is still limited by its low conductivity. The main reason is that the localized sp 3 Covalent bonds are not conducive to electron transport. It is generally believed that the electrical properties of diamond can be adjusted by doping. However, due to the low doping efficiency and high activation energy of dopants in diamond, it still cannot meet practical needs. Therefore, the development of new diamond-based materials with customized microstructures that can perfectly combine excellent mechanical properties and electrical properties is urgently needed for widespread application.
[0003] Compared with diamond, graphite is composed entirely of sp 2 The diamond matrix is a composite material obtained by introducing a graphite phase into a diamond matrix, thus showing high conductivity and ductility. Diamond composites obtained by introducing a graphite phase into a diamond matrix may be a feasible way to combine the advantages of both components. Recently, a new class of diamond-graphite nanocomposites such as diaphite and gradia structures with coherent interfaces have been identified from natural impact meteorites or synthesized under high pressure and high temperature (HPHT). The sp 2 Bonding graphite / graphene and sp 3 The bonded diamond hybrid units contribute to its excellent performance. In addition, compressing glassy carbon at high temperature (25GPa, 400-1200℃) can be transformed into bulk amorphous carbon with lightweight, hard and conductive properties. Recently, ultra-strong conductive carbon composites composed of ultrafine nanodiamonds embedded in a disordered multilayer graphene matrix with incoherent interfaces have been synthesized from glassy carbon at 25GPa and temperatures between 1050 and 1150℃. However, the industrial application of these carbon composites is still limited due to the small sample size (<2mm) mentioned above, which is restricted by the harsh synthesis conditions. Critical conditions are necessary because from the traditional sp 2 The transformation of carbon precursors into the diamond phase requires a high energy barrier. So far, centimeter-scale ultrahard and highly conductive diamond composites have not been achieved. Summary of the invention
[0004] In order to solve the above-mentioned problems and meet the characteristics of excellent processability and low manufacturing cost, the present invention provides a method for preparing centimeter-level super-tough, super-conductive and super-hard carbon composite materials.
[0005] The technical solution of the present invention is: a method for preparing a centimeter-level super-tough, super-conductive and super-hard carbon composite material, comprising the following steps;
[0006] Step 1: Removal of amorphous carbon on the surface of nanodiamond and pre-pressing
[0007] The bombarded nanodiamonds were heated to 450°C in air and kept at a constant temperature for 60 minutes to remove the amorphous carbon on the surface of the nanodiamonds, and then pre-pressed into a cylindrical block shape;
[0008] Step 2: Assembly
[0009] Place the cylindrical block obtained after step 1 into a zirconium / molybdenum cup, then place the zirconium / molybdenum cup into a salt tube, then place the salt tube into a graphite carbon mold, then place salt sheets on the top and bottom, then place carbon paper on the top and bottom of the outside of the salt sheets and install two hammers made of conductive polycrystalline diamond, and finally install a standard high-voltage assembly block.
[0010] Step 3: Heat and let stand to remove moisture
[0011] The standard high-pressure assembly block assembled in step 2 is heated to 115° C. in air and then kept at a constant temperature of 115° C. for 4 hours in order to remove moisture from the assembly.
[0012] Step 4: High temperature and high pressure treatment
[0013] The standard high-pressure assembly block completed in step 3 is loaded into a six-sided top press for high temperature and high pressure treatment.
[0014] Preferably, the graphite carbon mold in step 2 is prepared by using a three-impregnation and four-baking process graphite.
[0015] Preferably, the high temperature and high pressure treatment in step 4 is 1100-1500° C., the pressure is 7-12 GPa, and the maintenance time is 10-20 minutes.
[0016] Preferably, the purity of the bombarded nanodiamonds in step 1 is 99%, and the particle size is d, d≤5nm.
[0017] Preferably, in step 1, the material is pre-pressed into a cylindrical block with a diameter of 15.5 mm and a height of 4 mm.
[0018] Preferably, the six-sided top press in step 4 is a six-sided top industrial press with a cylinder diameter of 770 mm.
[0019] The beneficial effects of the present invention are:
[0020] The preparation method of the centimeter-level super-tough, super-conductive and super-hard carbon composite material of the present invention comprises the following steps: pre-pressing nano-diamonds into a cylindrical block shape by bombardment, sequentially loading the blocks into a special high-pressure assembly block by means of a salt pipe and a carbon mold, and then placing the high-pressure assembly block into a six-sided top press for high-temperature and high-pressure treatment. The particle size of the carbon composite block material prepared by the method is 13.4 mm-14.0 mm, reaching the centimeter level, and the Vickers hardness can reach 55.8 GPa, and the room-temperature conductivity can reach 2×10 4 Sm -1 , the fracture toughness can reach 19.8MPa m under a load of 19.8N 1 / 2 It has excellent conductivity, toughness and hardness, and its size reaches the centimeter level, which is higher than similar products in the existing technology, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the size distribution diagram of bombarded diamond after being treated at 450℃ / 60 minutes in air;
[0022] Figure 2 This is a high-resolution transmission electron microscope image of bombarded diamond after being treated at 450℃ / 60 minutes in air.
[0023] Figure 3 Selected diffraction patterns of bombarded diamond after treatment at 450°C / 60 minutes in air.
[0024] Figure 4 The carbon composite material block is synthesized under high temperature and high pressure in Example 1;
[0025] Figure 5 The carbon composite material block synthesized under high temperature and high pressure in Example 2;
[0026] Figure 6 Comparison of X-ray diffraction patterns of carbon composites synthesized in Examples 1 and 2 and bombarded nanodiamonds;
[0027] Figure 7 Comparison of Raman images of carbon composites synthesized in Examples 1 and 2 and bombarded nanodiamonds;
[0028] Figure 8 The high-resolution transmission electron microscope image and the corresponding diffraction pattern of the carbon composite material synthesized in Example 1;
[0029] Fig. 9 The high-resolution transmission electron microscope image and the corresponding diffraction pattern of the carbon composite material synthesized in Example 2;
[0030] Fig.10 Vickers hardness and indentation diagram of the carbon composite material synthesized in Examples 1 and 2;
[0031] Fig.11 is the room temperature conductivity curve of the carbon composite material synthesized in the example;
[0032] Fig.12 The thermogravimetric curve and differential thermal test curve of the carbon composite material synthesized in the example;
[0033] Fig.13 X-ray diffraction patterns of carbon composite bulk materials synthesized at 7 GPa pressure and 12 GPa pressure and temperature 1100-1500°C;
[0034] Fig.14 Raman images of carbon composite bulk synthesized at 7 GPa and 12 GPa pressures and temperatures of 1100-1500°C;
[0035] Fig.15 is a cross-sectional view of a high voltage component;
[0036] In the figure, 1. pyrophyllite, 2. carbon mold, 3. carbon tube or carbon sheet, 4. salt tube, 5. MgO cup, 6. steel cap, 7. hammer head, 8. cylindrical block with zirconium / molybdenum cup, 9. muscovite cup, 10. muscovite sheet. DETAILED DESCRIPTION
[0037] The specific implementation modes of the present invention are further described in detail below in conjunction with the embodiments.
[0038] Example 1
[0039] A method for preparing a centimeter-level super-tough, super-conductive and super-hard carbon composite material, comprising the following steps: Step 1: removing impurities from nanodiamonds and pre-pressing them into a shape
[0040] The purity of the bombarded nanodiamond with an average particle size of 99% and a particle size of d, d≤5nm, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., was selected; the bombarded nanodiamond was heated to 450°C in air, kept at a constant temperature for 60 minutes, amorphous carbon on the surface of the nanodiamond was removed, and then pre-pressed into a cylindrical block with a diameter of 15.5mm and a height of 4mm;
[0041] Step 2: Assembly
[0042] After completing step 1, the cylindrical block is placed in a zirconium / molybdenum cup. Fig.15 8, then put the zirconium / molybdenum cup into the salt tube 4, then put the salt tube into the graphite carbon mold 2, then put salt sheets on the top and bottom, then put carbon paper on the top and bottom of the salt sheet and put two hammer heads 7 made of conductive polycrystalline diamond, and finally put the standard high-voltage assembly block. In this step, the graphite carbon mold is prepared by three-impregnation and four-baking process graphite. The structural state after assembly is shown in FIG. Fig.15 As shown;
[0043] Step 3: Heat and let stand to remove moisture
[0044] The standard high-voltage assembly block assembled in step 2 is heated to 115°C in air, and then kept at a constant temperature of 115°C for 4 hours to remove moisture from the component to avoid the influence of moisture on the subsequent step 4.
[0045] Step 4: High temperature and high pressure treatment
[0046] The standard high-pressure assembly block completed in step 3 was loaded into a six-sided top press with a cylinder diameter of 770 mm for high temperature and high pressure treatment at a temperature of 1300°C and a pressure of 12 GPa for 15 minutes to obtain a carbon composite block. Figure 4 , whose size is much larger than the 10mm length comparison bar, which is 13.4mm-14.0mm.
[0047] The synthesized carbon composite bulk material was analyzed using an X-ray diffractometer, such as Figure 6 As shown, it can be seen that sp 2 and sp 3 Mixed phase structure; analyzed by Raman spectrometer (325nm excitation wavelength), such as Figure 7 As shown, it can be seen that the surface of the block has obvious sp 2 Carbon, judging the presence of sp in bulk materials by peak shape 3 Carbon; the bulk material was sampled by focused ion beam (FIB), and then observed by transmission electron microscopy high resolution and selected diffraction patterns ( Figure 8 ), it can be found that the sample contains a large number of graphite nanoribbons surrounding the diamond nanoparticles;
[0048] The above results consistently indicate that the samples contain sp 2 Carbon and sp 3 Diamond; Using Vickers hardness tester, the results show that the hardness of the synthetic sample at 1300℃ is 55.8GPa ( Fig.10 ), and its fracture toughness can reach 12.8MPa·m under a load of 19.6N by calculation. 1 / 2 (as shown in Table 1),
[0049] The temperature-dependent resistivity (such as Fig.11 The resistivity at room temperature is 2.0×10 4 S m -1 , by thermogravimetric analysis ( Fig.12 ) It can be seen that the initial carbonization temperature of the sample in air is 1005K, which is close to natural diamond. The above results show that the carbon composite material prepared by this method is a centimeter-scale, super-tough, super-conductive and super-hard block.
[0050] When the temperature in the high temperature and high pressure treatment step in Example 1 is adjusted to 1500° C., the hardness value of the synthesized sample is 40.2 GPa, and its fracture toughness can reach 19.8 MPa·m1 / 2 under a load of 19.6 N (as shown in Table 1).
[0051] Example 2: A method for preparing a centimeter-level ultra-tough, ultra-conductive, ultra-hard carbon composite material, comprising the following steps;
[0052] Step 1: Nanodiamond removal and pre-pressing
[0053] The purity of the bombarded nanodiamond with an average particle size of 99% and a particle size of d, d≤5nm, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., was selected; the bombarded nanodiamond was heated to 450°C in air, kept at a constant temperature for 60 minutes, amorphous carbon on the surface of the nanodiamond was removed, and then pre-pressed into a cylindrical block with a diameter of 15.5mm and a height of 4mm;
[0054] Step 2: Assembly
[0055] After completing step 1, the cylindrical block is placed in a zirconium / molybdenum cup. Fig.15 8, then put the zirconium / molybdenum cup into the salt tube 4, then put the salt tube into the graphite carbon mold 2, then put salt sheets on the top and bottom, then put carbon paper on the top and bottom of the salt sheet and put two hammer heads 7 made of conductive polycrystalline diamond, and finally put the standard high-voltage assembly block. In this step, the graphite carbon mold is prepared by three-impregnation and four-baking process graphite. The structural state after assembly is shown in FIG. Fig.15 As shown;
[0056] Step 3: Heat and let stand to remove moisture
[0057] Heat the standard high-voltage assembly block assembled in step 2 to 115°C in air and maintain a constant temperature of 115°C for 4 hours; the purpose is to remove moisture from the components to avoid the influence of moisture on the subsequent step 4.
[0058] Step 4: High temperature and high pressure treatment
[0059] The standard high-pressure assembly block completed in step 3 was loaded into a six-sided top press with a cylinder diameter of 770 mm for high temperature and high pressure treatment at a temperature of 1100°C and a pressure of 7 GPa for 15 minutes to obtain a carbon composite material block. Figure 5 , whose size is much larger than the 10mm length comparison bar, which is 13.4mm-14.0mm.
[0060] The synthesized carbon composite bulk material was analyzed using an X-ray diffractometer, such as Figure 6 As shown, it can be seen that sp 2 and sp 3Mixed phase structure; analyzed by Raman spectrometer (325nm excitation wavelength), such as Figure 7 As shown, it can be seen that the surface of the block has obvious sp 2 Carbon, judging the presence of sp in bulk materials by peak shape 3 Carbon; the bulk material was sampled by focused ion beam (FIB), and then observed by transmission electron microscopy high resolution and selected diffraction patterns ( Fig. 9 ), it can be found that the sample contains a large number of graphite nanoribbons surrounding the diamond nanoparticles; the above results consistently indicate that the sample contains sp 2 Carbon and sp 3 Diamond; tested with a Vickers hardness tester, the results show that the hardness value is 20GPa ( Fig.10 ), and its fracture toughness can reach 11.2MPa·m under a load of 19.6N by calculation. 1 / 2 .
[0061] The above results indicate that the carbon composite material prepared by this method is a centimeter-scale, super-tough, super-conductive and super-hard block.
[0062] Fig.13 and 14 The law that the strength of the obtained carbon composite material increases with the increase of pressure and synthesis temperature is given.
[0063] Table 1 Fracture toughness values of carbon composite materials synthesized in the examples
[0064]
Claims
1. A method for preparing a centimeter-level ultra-tough, ultra-conductive and ultra-hard carbon composite material, comprising the following steps; Step 1: Removal of amorphous carbon on the surface of nanodiamond and pre-pressing The bombarded nanodiamonds were heated to 450°C in air and kept at a constant temperature for 60 min to remove the amorphous carbon on the surface of the nanodiamonds, and then pre-pressed into a cylindrical block shape; Step 2: Assembly Place the cylindrical block obtained after step 1 into a zirconium / molybdenum cup, then place the zirconium / molybdenum cup into a salt tube, then place the salt tube into a graphite carbon mold, then place salt sheets on the top and bottom, then place carbon paper on the top and bottom of the salt sheets and install two hammers made of conductive polycrystalline diamond, and finally install a standard high-voltage assembly block; Step 3: Heat and let stand to remove moisture The standard high-voltage assembly block assembled in step 2 is heated to 115°C in air, and then kept at a constant temperature of 115°C for 4 hours to remove moisture from the assembly; Step 4: High temperature and high pressure treatment Load the standard high-pressure assembly block completed in step 3 into a six-sided top press for high-temperature and high-pressure treatment; The high temperature and high pressure treatment in step 4 is 1100-1500 °C, the pressure is 7-12 GPa, and the holding time is 10-20 minutes.
2. The method for preparing the centimeter-level ultra-tough, ultra-conductive and ultra-hard carbon composite material according to claim 1, characterized in that: The graphite carbon mold in step 2 is prepared by using a three-impregnation and four-baking process.
3. The method for preparing the centimeter-level ultra-tough, ultra-conductive and ultra-hard carbon composite material according to claim 1, characterized in that: The purity of the bombarded nanodiamonds in step 1 is 99%, and the particle size is d, d≤5 nm.
4. The method for preparing centimeter-level ultra-tough, ultra-conductive and ultra-hard carbon composite material according to claim 1, characterized in that: In step 1, the material is pre-pressed into a cylindrical block with a diameter of 15.5 mm and a height of 4 mm.
5. The method for preparing centimeter-level ultra-tough, ultra-conductive and ultra-hard carbon composite material according to claim 1, characterized in that: The six-sided top press in step 4 is a six-sided top industrial press with a cylinder diameter of 770 mm.