Anti-aging auxiliary agent composition and preparation method thereof
By adding antioxidants, functional additives and other components to polycarbonate materials, an anti-aging additive composition with hydrophobicity and multi-scale cross-linked network structure is prepared, which solves the problem of poor anti-aging effect in the prior art and achieves high efficiency in thermal stability and UV resistance of the material.
Patent Information
- Application Number
- CN202311016527.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-14
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-08-14
AI Technical Summary
Existing anti-aging additive compositions have poor solubility in polycarbonate materials, resulting in poor resistance to ultraviolet radiation and high-temperature thermal aging, and unstable material properties.
An anti-aging additive composition with hydrophobic and multi-scale cross-linked network structure was prepared by using antioxidants, functional additives, antistatic agents, compatibilizers and dispersants, which were mixed in a high-speed mixer and then extruded, cooled and pelletized in a twin-screw extruder.
It significantly improves the thermal stability and UV resistance of polycarbonate materials, enhances their toughness and strength, slows down the aging rate, and improves their weather resistance and durability.
Smart Images

Figure BDA0004392082450000101 
Figure BDA0004392082450000102
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite materials, and in particular to an anti-aging auxiliary composition and a preparation method thereof. Background Art
[0002] In the prior art, the anti-aging additive composition of polycarbonate (PC) mainly includes an anti-aging additive composition, which includes three components, namely, an antioxidant, an ultraviolet absorber and a light stabilizer. The composition can effectively improve the weather resistance and durability of polycarbonate materials and extend the service life of the material. The functional anti-aging additive composition, which includes components such as antioxidants, ultraviolet absorbers and plasticizers, has excellent antioxidant properties, ultraviolet stability and plasticizing effects, can improve the toughness and strength of polycarbonate materials and extend the service life of the material. The high-efficiency anti-aging additive composition, which includes components such as antioxidants, ultraviolet absorbers, light stabilizers and plasticizers, can effectively improve the weather resistance, durability, antioxidant properties and plasticizing effects of PC materials, and also has good dispersibility and stability. The anti-aging additive composite, which includes components such as antioxidants, ultraviolet absorbers, light stabilizers and plasticizers, can effectively improve the weather resistance, durability, antioxidant properties and plasticizing effects of polycarbonate materials, and also has certain fire resistance and chemical resistance.
[0003] However, these compositions still have some disadvantages in practical applications. The application scope of different compositions is limited, and the anti-aging effect on polycarbonate materials is poor or ineffective. The solubility in polycarbonate is poor and it cannot be evenly dispersed in the material, resulting in unstable material performance and low anti-ultraviolet and high-temperature thermal aging effects.
[0004] The present invention aims at some shortcomings and deficiencies of these compositions and makes further improvements and optimizations.
[0005] Invention patent application CN116102785A discloses a PC anti-aging agent and a preparation method thereof, and relates to the technical field of PC additives; wherein, the PC anti-aging agent, in terms of weight, comprises: 8 to 17 parts of antioxidant, 2 to 5 parts of functional combination additive, 0.1 to 0.5 parts of anti-yellowing agent, 0.5 to 1.5 parts of nucleating agent, 1 to 3 parts of mildewproof agent, 10 to 15 parts of dispersant and 40 to 45 parts of resin. The PC anti-aging agent has good compatibility with the matrix polycarbonate, and can be effectively dispersed in the polycarbonate in the hot melt state, improving the polycarbonate's resistance to all-weather aging, including ultraviolet light aging and thermal temperature aging. However, the PC anti-aging agent prepared by the invention does not add effective anti-aging additives, and still has the disadvantages of poor anti-ultraviolet and thermal aging performance. Summary of the invention
[0006] In view of the disadvantages of poor anti-ultraviolet and heat aging performance of the anti-aging auxiliary composition in the prior art, the technical problem to be solved by the present invention is to provide an anti-aging auxiliary composition with good anti-ultraviolet and heat aging performance and a preparation method thereof.
[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0008] An anti-aging auxiliary composition comprises the following raw materials: an antioxidant, a functional combination auxiliary, an antistatic agent, a compatibilizer, a dispersant and a resin.
[0009] Preferably, the anti-aging auxiliary agent composition comprises the following raw materials in parts by weight: 2 to 4 parts of antioxidant, 1 to 3 parts of functional combination auxiliary agent, 0.1 to 1 part of antistatic agent, 0.5 to 1 part of compatibilizer, 0.2 to 0.6 part of dispersant, and 50 to 70 parts of resin.
[0010] A method for preparing an anti-aging auxiliary composition is as follows:
[0011] Step 1, weighing each raw material according to weight, mixing the antioxidant, functional combination auxiliary agent, antistatic agent, compatibilizer, dispersant and resin in a high-speed mixer at a temperature of 50 to 60° C. and a rotation speed of 200 to 300 rpm to obtain a mixed material;
[0012] Step 2, putting the mixed material obtained in step 1 into a twin-screw extruder, extruding, cooling, and pelletizing to obtain pellets; the extrusion end temperature of the twin-screw extruder is 210-230° C., the main engine speed is 50-150rpm, the melt pressure is 1-3MPa, and the outlet pressure is 5-10MPa;
[0013] Step 3: Dry the pellets obtained in step 2 at 50-70° C. for 1-3 hours to obtain an anti-aging auxiliary composition.
[0014] The antioxidant is at least one of tris(2,4-di-tert-butylphenyl)phosphite, butylated hydroxyanisole, butylated hydroxytoluene, tert-butylhydroquinone, diphenylamine and p-phenylenediamine.
[0015] The antistatic agent is at least one of octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate, polyethylene wax grafted sodium acrylate, and hexadecanol sulfate methyl salt.
[0016] The compatibilizer is at least one of maleic anhydride grafted polyethylene and silane coupling agent KH550.
[0017] The dispersant is at least one of polyethylene wax, N,N'-ethylenebisstearamide, 1-ethyl-3-methylimidazole chloride, dibutyltin dichloride, and hexamethylphosphoric triamide.
[0018] The resin is at least one of POE resin, polystyrene, and ethylene-ethyl acrylate copolymer.
[0019] The preparation method of the functional combination auxiliary agent is as follows, in parts by weight:
[0020] S1, heating 70-90 parts of water to 70-90° C., then dripping a pre-emulsion at a dripping speed of 1-3 mL / min, wherein the pre-emulsion consists of 4-6 parts of methyl methacrylate, 0.5-2 parts of ammonium persulfate, and 1-3 parts of sodium dodecyl sulfate, and stirring the mixture at 100-300 rpm for 30-50 min to obtain an emulsion;
[0021] S2, adding 4 to 6 parts of titanium dioxide to 70 to 90 parts of water, stirring at 100 to 500 rpm for 1 to 5 hours to obtain a dispersion, adding 0.5 to 2 parts of 2,2'-azobisisobutylamidine dihydrochloride to the dispersion, stirring at 100 to 300 rpm for reaction for 10 to 30 minutes, then adding the emulsion prepared in step S1, heating to 60 to 70°C and maintaining for 0.5 to 2 hours, adding 0.5 to 1 part of polyethylene glycol monooctylphenyl ether, heating to 60 to 80°C and maintaining for 10 to 20 minutes, then heating to 75 to 85°C, stirring at 100 to 500 rpm for 10 to 30 minutes, cooling to room temperature, adding 0.3 to 0.8 parts of 3-trimethylsiloxypropanol and 0.4 to 0.8 parts of dodecyltrimethoxysilane, maintaining at 70 to 90°C for 0.5 to 3 hours, and drying at room temperature for 20 to 30 hours to obtain a pretreated product;
[0022] S3, adding 1 to 3 parts of the pretreated material prepared in step S2 to 150 to 250 parts of 0.4 to 0.6 wt% ethanol solution of tridecafluorooctyltrimethoxysilane, adding 5 to 15 parts of water, 0.5 to 1 part of 2-chloroethyl vinyl ether, and 0.5 to 1 part of carbon nanotubes, ultrasonically treating at room temperature for 10 to 30 minutes, with an ultrasonic power of 50 to 300 W and an ultrasonic frequency of 40 to 60 kHz, stirring at 100 to 500 rpm for 5 to 15 hours, and drying at 60 to 90° C. to obtain a functional combination auxiliary agent.
[0023] The antioxidant used in the present invention is tris(2,4-di-tert-butylphenyl)phosphite, which can effectively inhibit the oxidation reaction of the polycarbonate material under light, heat and other environments, thereby extending the service life of the material.
[0024] Functional combination additives have a steric stabilization effect. Due to the synergistic effect of hydrophobicity and multi-scale cross-linked network structure, they have extremely strong water repellency and outstanding self-cleaning and anti-fouling properties. They can effectively resist the penetration of oxidizing substances, slow down the aging rate, and improve the UV resistance and thermal stability of polycarbonate materials. At the same time, they also have a good plasticizing effect, which can improve the toughness and strength of the material, thereby slowing down the aging process of polycarbonate materials.
[0025] Octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate is an ionic surfactant that can effectively increase the surface tension and dispersibility of polycarbonate materials, thereby enhancing the weather resistance and durability of polycarbonate materials.
[0026] The dispersant can improve the dispersibility and stability of the mixed material, avoid deformation or stratification of the material due to stress, and thus ensure the uniformity and stability of the anti-aging additive composition during the extrusion and molding process.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] 1) The anti-aging auxiliary composition prepared by adding a functional combination auxiliary agent in the present invention can significantly improve the thermal stability when used in polycarbonate. Due to the synergistic effect of hydrophobicity and multi-scale cross-linked network structure, it has extremely strong water repellency and outstanding self-cleaning and anti-fouling properties, can effectively resist the penetration of oxidizing substances, and slow down the aging rate.
[0029] 2) The antioxidant, functional combination auxiliary agent, antistatic agent, compatibilizer and dispersant in the present invention can work synergistically and be applied in polycarbonate materials to improve the heat resistance, UV resistance and oxidation resistance of polycarbonate materials, slow down the aging process of materials, and improve the toughness and strength of materials. DETAILED DESCRIPTION
[0030] Main sources of substances:
[0031] Polystyrene: Item No.: 3235, Jiangsu Qinghe Chemical Co., Ltd.
[0032] Titanium dioxide: Crystal form: rutile, Anhui Kerun Nanotechnology Co., Ltd.
[0033] Polycarbonate: Jiangsu Changfu Plastic Chemical Co., Ltd., item number: 2805.
[0034] Polyethylene glycol monooctylphenyl ether: Wuhan Kemik Biopharmaceutical Technology Co., Ltd., model: Triton X-100.
[0035] Carbon nanotubes: Xuzhou Jie Innovation Materials Technology Co., Ltd., fineness: 2nm, length: 1-2um.
[0036] Maleic anhydride grafted polyethylene: Guangzhou Zhongjie Chemical Technology Co., Ltd., brand: ZJ-900E.
[0037] Example 1
[0038] A method for preparing an anti-aging auxiliary composition is as follows:
[0039] Step 1, 3 kg of tris(2,4-di-tert-butylphenyl) phosphite, 1.5 kg of functional combination auxiliary agent, 0.5 kg of octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate, 0.8 kg of maleic anhydride grafted polyethylene, 0.4 kg of N,N'-ethylene bisstearamide and 60 kg of polystyrene are mixed in a high-speed mixer at a temperature of 55° C. and a rotation speed of 250 rpm to obtain a mixed material;
[0040] Step 2, putting the mixed material obtained in step 1 into a twin-screw extruder, extruding, cooling, and pelletizing to obtain pellets; the extrusion end temperature of the twin-screw extruder is 220° C., the main engine speed is 100 rpm, the melt pressure is 2 MPa, and the outlet pressure is 8 MPa;
[0041] Step 3: Place the pellets obtained in step 2 in an oven and dry at 60° C. for 2 h to obtain an anti-aging auxiliary composition.
[0042] The preparation method of the functional combination auxiliary agent is as follows:
[0043] S1, heat 80g of water to 80°C, then drop the pre-emulsion into the mixture at a dropping speed of 2mL / min, wherein the pre-emulsion consists of 5g of methyl methacrylate, 1g of ammonium persulfate, and 2g of sodium dodecyl sulfate, and stir at 200rpm for 40min to obtain an emulsion;
[0044] S2, adding 5g of titanium dioxide to 80g of water, stirring at 300rpm for 3h to obtain a dispersion, adding 1g of 2,2'-azobisisobutylamidine dihydrochloride to the dispersion, stirring at 200rpm for 20min, then adding the emulsion prepared in step S1, heating to 65°C for 1h, adding 0.8g of polyethylene glycol monooctylphenyl ether, heating to 70°C for 15min, then heating to 82°C, stirring at 200rpm for 20min, cooling to room temperature, adding 0.5g of 3-trimethylsiloxypropanol and 0.6g of dodecyltrimethoxysilane, keeping at 80°C for 1h, and drying at room temperature for 24h to obtain a pretreated product;
[0045] S3. Add 2 g of the pretreated material prepared in step S2 to 200 g of a 0.5 wt% ethanol solution of tridecafluorooctyltrimethoxysilane, add 10 g of water, 0.8 g of 2-chloroethyl vinyl ether, and 0.7 g of carbon nanotubes, perform ultrasonic treatment at 300 W for 20 min at room temperature, with an ultrasonic power of 200 W and an ultrasonic frequency of 50 kHz, stir at 300 rpm for 12 h, and then dry at 80° C. to obtain a functional combination additive.
[0046] Example 2
[0047] The preparation method of an anti-aging auxiliary agent composition is basically the same as that of Example 1, the only difference being that the preparation method of the functional combination auxiliary agent is different.
[0048] The preparation method of the functional combination auxiliary agent is as follows:
[0049] S1, heat 80g of water to 80°C, then drop the pre-emulsion into the mixture at a dropping speed of 2mL / min, wherein the pre-emulsion consists of 5g of methyl methacrylate, 1g of ammonium persulfate, and 2g of sodium dodecyl sulfate, and stir at 200rpm for 40min to obtain an emulsion;
[0050] S2, adding 5g of titanium dioxide to 80g of water, stirring at 300rpm for 3h to obtain a dispersion, adding 1g of 2,2'-azobisisobutylamidine dihydrochloride to the dispersion, stirring at 200rpm for 20min, then adding the emulsion prepared in step S1, heating to 65°C for 1h, adding 0.8g of polyethylene glycol monooctylphenyl ether, heating to 70°C for 15min, then heating to 82°C, stirring at 200rpm for 20min, cooling to room temperature, adding 0.5g of 3-trimethylsiloxypropanol, keeping at 80°C for 1h, and drying at room temperature for 24h to obtain a pretreated product;
[0051] S3. Add 2 g of the pretreated material prepared in step S2 to 200 g of a 0.5 wt% ethanol solution of tridecafluorooctyltrimethoxysilane, add 10 g of water, 0.8 g of 2-chloroethyl vinyl ether, and 0.7 g of carbon nanotubes, perform ultrasonic treatment at 300 W for 20 min at room temperature, with an ultrasonic power of 200 W and an ultrasonic frequency of 50 kHz, stir at 300 rpm for 12 h, and then dry at 80° C. to obtain a functional combination additive.
[0052] Example 3
[0053] The preparation method of an anti-aging auxiliary agent composition is basically the same as that of Example 1, the only difference being that the preparation method of the functional combination auxiliary agent is different.
[0054] The preparation method of the functional combination auxiliary agent is as follows:
[0055] S1, heat 80g of water to 80°C, then drop the pre-emulsion into the mixture at a dropping speed of 2mL / min, wherein the pre-emulsion consists of 5g of methyl methacrylate, 1g of ammonium persulfate, and 2g of sodium dodecyl sulfate, and stir at 200rpm for 40min to obtain an emulsion;
[0056] S2, adding 5g of titanium dioxide to 80g of water, stirring at 300rpm for 3h to obtain a dispersion, adding 1g of 2,2'-azobisisobutylamidine dihydrochloride to the dispersion, stirring at 200rpm for 20min, then adding the emulsion prepared in step S1, heating to 65°C for 1h, adding 0.8g of polyethylene glycol monooctylphenyl ether, heating to 70°C for 15min, then heating to 82°C, stirring at 200rpm for 20min, cooling to room temperature, adding 0.5g of 3-trimethylsiloxypropanol and 0.6g of dodecyltrimethoxysilane, keeping at 80°C for 1h, and drying at room temperature for 24h to obtain a pretreated product;
[0057] S3. Add 2 g of the pretreated material prepared in step S2 to 200 g of anhydrous ethanol, add 10 g of water, 0.8 g of 2-chloroethyl vinyl ether, and 0.7 g of carbon nanotubes, and perform ultrasonic treatment at 300 W for 20 min at room temperature, with an ultrasonic power of 200 W and an ultrasonic frequency of 50 kHz. Stir at 300 rpm for 12 h, and then dry at 80° C. to obtain a functional combination additive.
[0058] Example 4
[0059] The preparation method of an anti-aging auxiliary agent composition is basically the same as that of Example 1, the only difference being that the preparation method of the functional combination auxiliary agent is different.
[0060] The preparation method of the functional combination auxiliary agent is as follows:
[0061] S1, heat 80g of water to 80°C, then drop the pre-emulsion into the mixture at a dropping speed of 2mL / min, wherein the pre-emulsion consists of 5g of methyl methacrylate, 1g of ammonium persulfate, and 2g of sodium dodecyl sulfate, and stir at 200rpm for 40min to obtain an emulsion;
[0062] S2, adding 5g of titanium dioxide to 80g of water, stirring at 300rpm for 3h to obtain a dispersion, adding 1g of 2,2'-azobisisobutylamidine dihydrochloride to the dispersion, stirring at 200rpm for 20min, then adding the emulsion prepared in step S1, heating to 65°C for 1h, adding 0.8g of polyethylene glycol monooctylphenyl ether, heating to 70°C for 15min, then heating to 82°C, stirring at 200rpm for 20min, cooling to room temperature, adding 0.5g of 3-trimethylsiloxypropanol and 0.6g of dodecyltrimethoxysilane, keeping at 80°C for 1h, and drying at room temperature for 24h to obtain a pretreated product;
[0063] S3. Add 2 g of the pretreated material prepared in step S2 to 200 g of a 0.5 wt% ethanol solution of tridecafluorooctyltrimethoxysilane, add 10 g of water and 0.8 g of 2-chloroethyl vinyl ether, perform ultrasonic treatment at 300 W for 20 min at room temperature, with an ultrasonic power of 200 W and an ultrasonic frequency of 50 kHz, stir at 300 rpm for 12 h, and then dry at 80° C. to obtain a functional combination additive.
[0064] Comparative Example 1
[0065] The preparation method of an anti-aging auxiliary agent composition is basically the same as that of Example 1, the only difference being that the preparation method of the functional combination auxiliary agent is different.
[0066] The preparation method of the functional combination auxiliary agent is as follows:
[0067] S1, heat 80g of water to 80°C, then drop the pre-emulsion into the mixture at a dropping speed of 2mL / min, wherein the pre-emulsion consists of 5g of methyl methacrylate, 1g of ammonium persulfate, and 2g of sodium dodecyl sulfate, and stir at 200rpm for 40min to obtain an emulsion;
[0068] S2, adding 5g of titanium dioxide to 80g of water, stirring at 300rpm for 3h to obtain a dispersion, adding 1g of 2,2'-azobisisobutylamidine dihydrochloride to the dispersion, stirring at 200rpm for 20min, then adding the emulsion prepared in step S1, heating to 65°C for 1h, adding 0.8g of polyethylene glycol monooctylphenyl ether, heating to 70°C for 15min, then heating to 82°C, stirring at 200rpm for 20min, cooling to room temperature, adding 0.5g of 3-trimethylsiloxypropanol, keeping at 80°C for 1h, and drying at room temperature for 24h to obtain a pretreated product;
[0069] S3. Add 2 g of the pretreated material prepared in step S2 to 200 g of anhydrous ethanol, add 10 g of water and 0.8 g of 2-chloroethyl vinyl ether, perform ultrasonic treatment at 300 W for 20 min at room temperature, with an ultrasonic power of 200 W and an ultrasonic frequency of 50 kHz. Stir at 300 rpm for 12 h, and then dry at 80° C. to obtain a functional combination additive.
[0070] Comparative Example 2
[0071] A method for preparing an anti-aging auxiliary composition is as follows:
[0072] Step 1, 3 kg of tris(2,4-di-tert-butylphenyl) phosphite, 0.5 kg of octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate, 0.8 kg of maleic anhydride grafted polyethylene, 0.4 kg of N,N'-ethylene bisstearamide and 60 kg of polystyrene are mixed in a high-speed mixer at a temperature of 55° C. and a rotation speed of 250 rpm to obtain a mixed material;
[0073] Step 2, putting the mixed material obtained in step 1 into a twin-screw extruder, extruding, cooling, and pelletizing to obtain pellets; the extrusion end temperature of the twin-screw extruder is 220° C., the main engine speed is 100 rpm, the melt pressure is 2 MPa, and the outlet pressure is 8 MPa;
[0074] Step 3: Place the pellets obtained in step 2 in an oven and dry at 60° C. for 2 h to obtain an anti-aging auxiliary composition.
[0075] Test Example 1
[0076] Light aging test
[0077] The polycarbonate pellets were dried in an oven at 120° C. overnight, the dried raw materials and modified titanium dioxide were weighed according to the mass ratio, 5 wt % of the anti-aging auxiliary composition was added and mixed thoroughly in a high-speed mixer.
[0078] After the polycarbonate pellets and the anti-aging additive composition are mixed, they are melt-extruded through a twin-screw extruder, and the solidified raw materials are converted into a uniform viscous fluid through heating and mixing of the extruder; they are extruded and granulated according to a conventional extrusion process, and the blend after extrusion and granulation is dried in an oven at 50°C for 5 hours, and processed into standard tensile specimens by injection molding using an injection machine in accordance with GB / T1040.2-2022 "Determination of Tensile Properties of Plastics Part 2: Test Conditions for Molded and Extruded Plastics".
[0079] Four specimens were prepared for each group, and the standard tensile specimens were irradiated under 50W ultraviolet light for 10 days in a ventilated environment.
[0080] Tensile performance test: Place the samples before and after aging in the two fixtures of the testing machine, so that the longitudinal axis of the sample coincides with the center line of the upper and lower fixtures, and maintain a certain degree of tightness so that the sample will not slip out or break in the fixture; start the tensile test at a tensile rate of 30mm / min until the sample breaks, and read the tensile strength from the computer;
[0081] Each group was tested three times and the average value was taken. The test results are shown in Table 1.
[0082] Table 1: Light aging test results
[0083]
[0084] Test Example 2
[0085] Damp heat aging test
[0086] The sample prepared in Test Example 1 was placed in a wet heat aging test box (GSJ-100B, Shanghai Suying Testing Instrument Co., Ltd.), aged for 300 hours at a temperature of 85° C. and a humidity of 85%, and then the tensile properties were tested using the method of Test Example 1.
[0087] Each group was tested three times and the average value was taken. The test results are shown in Table 2.
[0088] Table 2: Damp heat aging test results
[0089]
[0090] It can be seen from the test results of test examples 1 to 2 that the anti-aging auxiliary agent composition of Example 1 has the best effect on the light aging and wet-heat aging of PC materials. The possible reason is that in Example 1 of the present invention, tris(2,4-di-tert-butylphenyl) phosphite, functional combination auxiliary agent, octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate, maleic anhydride grafted polyethylene, N,N'-ethylene bisstearamide and polystyrene are mixed and granulated to obtain the anti-aging auxiliary agent composition. The functional combination auxiliary agent is prepared by heating water, then dripping a pre-emulsion consisting of methyl methacrylate, ammonium persulfate and sodium dodecyl sulfate, stirring and reacting to obtain an emulsion; adding titanium dioxide into water and stirring to obtain a dispersion, adding 2,2'-azobisisobutylamidine dihydrochloride into the dispersion and stirring and reacting, then adding the emulsion, heating, adding polyethylene glycol monooctylphenyl ether, heating, stirring, cooling to room temperature, adding 3-trimethylsiloxypropanol and dodecyltrimethoxysilane, reacting at high temperature, drying to obtain a pretreated product; adding the pretreated product into an ethanol solution of tridecafluorooctyltrimethoxysilane, adding water, 2-chloroethyl vinyl ether and carbon nanotubes, ultrasonically treating, stirring, and drying to obtain the functional combination auxiliary agent.
[0091] The latex molecules can form hydrogen bonds with the -OH groups on the surface of the titanium dioxide particles, and due to the hydrophobic interaction between the organic parts of the latex molecules, they attract each other, resulting in the agglomeration of the titanium dioxide particles. After the titanium dioxide particles are modified with dodecyltrimethoxysilane, the size of the agglomerated titanium dioxide particles is reduced and the agglomeration is reduced. Since dodecyltrimethoxysilane has a low self-condensation, it has a steric stabilizing effect between the titanium dioxide particles. In addition, the modification of the titanium dioxide particles reduces the transparency of the polycarbonate and improves the UV resistance and thermal stability of the polycarbonate material.
[0092] The modified titanium dioxide particles can reduce the permeability of volatile products formed by thermal decomposition in the polymer, thereby reducing the possibility of oxidation reactions, thereby playing a role in heat insulation and oxygen isolation. Furthermore, since the pretreated material has excellent hydrophobicity after being modified with tridecafluorooctyltrimethoxysilane, 2-chloroethyl vinyl ether, as a complex and strong adhesive, can improve the binding ability of the functional combination additive with polycarbonate, and carbon nanotubes and pretreated materials are conducive to promoting crosslinking inside polycarbonate. The addition of functional combination additives increases the interaction between the functional combination additives and polycarbonate, thereby limiting the mobility of polycarbonate chains, preventing chain breakage in polycarbonate, and significantly improving the thermal stability of polycarbonate. Due to the synergistic effect of hydrophobicity and multi-scale cross-linked network structure, it has extremely strong water repellency and outstanding self-cleaning and anti-fouling properties, can effectively resist the penetration of oxidizing substances, and slow down the aging rate.
Claims
1. An anti-aging auxiliary composition, It is characterized in that The composition comprises the following raw materials in parts by weight: 2 to 4 parts of antioxidant, 1 to 3 parts of functional combination additive, 0.1 to 1 part of antistatic agent, 0.5 to 1 part of compatibilizer, 0.2 to 0.6 part of dispersant, and 50 to 70 parts of resin; The preparation method of the functional combination auxiliary agent is as follows, in parts by weight: S1, heating 70-90 parts of water to 70-90° C., then dripping a pre-emulsion at a dropping speed of 1-3 mL / min, wherein the pre-emulsion consists of 4-6 parts of methyl methacrylate, 0.5-2 parts of ammonium persulfate, and 1-3 parts of sodium dodecyl sulfate, and stirring the mixture at 100-300 rpm for 30-50 min to obtain an emulsion; S2, adding 4-6 parts of titanium dioxide to 70-90 parts of water, stirring at 100-500rpm for 1-5h to obtain a dispersion, adding 0.5-2 parts of 2,2'-azobisisobutylamidine dihydrochloride to the dispersion, stirring and reacting at 100-300rpm for 10-30min, then adding the emulsion prepared in step S1, heating to 60-70°C and keeping for 0.5-2h, adding 0.5-1 parts of polyethylene glycol monooctylphenyl ether, heating to 60-80°C and keeping for 10-20min, then heating to 75-85°C, stirring at 100-500rpm for 10-30min, cooling to room temperature, adding 0.3-0.8 parts of 3-trimethylsiloxypropanol and 0.4-0.8 parts of dodecyltrimethoxysilane, keeping at 70-90°C for 0.5-3h, and drying at room temperature for 20-30h to obtain a pretreated product; S3, adding 1 to 3 parts of the pretreated material prepared in step S2 to 150 to 250 parts of an ethanol solution of 0.4 to 0.6 wt % tridecafluorooctyltrimethoxysilane, adding 5 to 15 parts of water, 0.5 to 1 part of 2-chloroethyl vinyl ether, and 0.5 to 1 part of carbon nanotubes, ultrasonically treating at room temperature for 10 to 30 min, with an ultrasonic power of 50 to 300 W and an ultrasonic frequency of 40 to 60 kHz, stirring at 100 to 500 rpm for 5 to 15 h, and drying at 60 to 90° C. to obtain a functional combination additive; The antioxidant is at least one of tris(2,4-di-tert-butylphenyl)phosphite, butylated hydroxyanisole, butylated hydroxytoluene, tert-butylhydroquinone, diphenylamine, and p-phenylenediamine; The antistatic agent is at least one of octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate and polyethylene wax grafted sodium acrylate; The compatibilizer is at least one of maleic anhydride grafted polyethylene and silane coupling agent KH550; The dispersant is at least one of polyethylene wax, N,N'-ethylenebisstearamide, 1-ethyl-3-methylimidazole chloride, dibutyltin dichloride, and hexamethylphosphoric triamide; The resin is at least one of POE resin, polystyrene, and ethylene-ethyl acrylate copolymer.
2. A method for preparing the anti-aging auxiliary composition as claimed in claim 1, It is characterized in that The preparation method is as follows: Step 1, weighing each raw material according to weight, mixing the antioxidant, functional combination additive, antistatic agent, compatibilizer, dispersant and resin in a high-speed mixer at a temperature of 50-60° C. and a rotation speed of 200-300 rpm to obtain a mixed material; Step 2, putting the mixed material obtained in step 1 into a twin-screw extruder, extruding, cooling, and pelletizing to obtain pellets; the extrusion end temperature of the twin-screw extruder is 210-230° C., the main engine speed is 50-150rpm, the melt pressure is 1-3MPa, and the outlet pressure is 5-10MPa; Step 3: Dry the pellets obtained in step 2 at 50-70° C. for 1-3 hours to obtain an anti-aging auxiliary composition.