Water-soluble temporary plugging agent for oil well fracturing and preparation method thereof

By combining the modified polyaspartic acid polymer with acrylamide, a water-soluble temporary plugging agent is formed, which solves the problem of poor solubility of acrylamide polymers in the prior art, and improves the sealing ability and dissolution speed of oil well fracturing. Achieve more efficient oil well development results.

CN117126340BActive Publication Date: 2024-11-01XIAN CHUAN QIN SHIYOU SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310862657.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-14
Publication Date
2024-11-01
Estimated Expiration
2043-07-14

AI Technical Summary

Technical Problem

The existing oil well temporary plugging agents, especially acrylamide polymers, have poor solubility and are difficult to meet the performance requirements of water-soluble temporary plugging agents in oil well fracturing.

Method used

Modified polyaspartic acid polymer is used to bind to acrylamide, and a water-soluble temporary plugging agent is formed through covalent linking reaction, which improves its dissolution rate in water and rock binding performance.

Benefits of technology

The sealing ability and dissolution speed of temporary plugging agent are improved, the binding performance with rock is enhanced, the problem of poor solubility of acrylamide polymer is solved, and a more efficient oil well fracturing effect is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a water-soluble temporary plugging agent for oil well fracturing and a preparation method thereof, which relate to the technical field of plugging agents. The water-soluble temporary plugging agent comprises the following raw materials in parts by weight: 20-30 parts of acrylamide, 15-25 parts of modified polyaspartic acid polymer, 0.1-0.2 parts of potassium persulfate and 50-70 parts of deionized water; polyacrylamide is used as a main material, and the modified polyaspartic acid polymer is used to construct a water-absorbing and swelling material; the modified polyaspartic acid polymer has the water solubility of polyaspartic acid itself, and contains amino groups and the like in the molecule, and is easy to adhere to the rock surface through hydrogen bonds; thereby further improving the combining performance of the prepared modified polyaspartic acid polymer with the rock, and improving the plugging ability of the temporary plugging agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plugging agents, and in particular to a water-soluble temporary plugging agent for oil well fracturing and a preparation method thereof. Background Art

[0002] The horizontal well open hole staged fracturing transformation technology for tight sandstone reservoirs has been improved and widely promoted and applied, making great contributions to the efficient development of low permeability tight sandstone. However, with the deepening of development and the increase in demand for oil and natural gas, maximizing production while reducing construction risks and difficulties has become the direction of our continued in-depth efforts, such as realizing multi-fracture fracturing in open hole horizontal wells to increase the transformation volume of the reservoir.

[0003] Through the technology of temporary plugging multiple fractures in horizontal well sections, temporary plugging agents are used to produce filter cake bridge plugging in high permeability zones, forming a pressure difference value higher than the fracture pressure of the upper fracture, which promotes the formation of new fractures. In this way, multiple fractures in the horizontal well section can be fractured, the fracture density in the horizontal section can be increased, the reserves of the horizontal well can be further increased, the regional volume transformation can be achieved, and the gas well production can be increased.

[0004] Currently common temporary plugging agents can be roughly divided into the following categories: acid fracturing temporary plugging agents, cross-linking and gel-breaking temporary plugging agents, and water-swelling temporary plugging agents. The key indicators of a good temporary plugging agent are high plugging ability before dissolution and a suitable dissolution rate. However, acrylamide polymers have poor solubility. Therefore, how to provide a water-soluble temporary plugging agent with excellent performance is a technical problem that needs to be solved urgently. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a water-soluble temporary plugging agent for oil well fracturing and a preparation method thereof.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A water-soluble temporary plugging agent for oil well fracturing, comprising the following raw materials in parts by weight: 20-30 parts of acrylamide, 15-25 parts of modified polyaspartic acid polymer, 0.1-0.2 parts of potassium persulfate, and 50-70 parts of deionized water;

[0008] The water-soluble temporary plugging agent for oil well fracturing comprises the following steps:

[0009] Acrylamide and modified polyaspartic acid polymer were added into deionized water, heated to 60°C, stirred at a uniform speed and reacted for 1 hour, then potassium persulfate was added, kept warm and reacted for 12 hours, filtered and dried after the reaction was completed, and a water-soluble temporary plugging agent for oil well fracturing was obtained.

[0010] Further: the modified polyaspartic acid polymer comprises the following steps:

[0011] Step S1, adding L-aspartic acid and 85% by mass phosphoric acid into a three-necked flask, heating to 180° C. and reacting under reduced pressure for 2.5 hours, then cooling to room temperature, dissolving with N,N-dimethylformamide and filtering, placing the filtrate in deionized water and stirring at a constant speed for 1 hour, suction filtering, washing the filter cake with deionized water until the washing liquid is neutral, and then vacuum drying at 55° C. to obtain polyaspartic acid;

[0012] Step S2, adding the prepared polyaspartic acid into a three-necked flask filled with N,N-dimethylformamide, introducing nitrogen, magnetically stirring in an ice-water bath and slowly dropping a solution of ethanolamine in N,N-dimethylformamide, continuing to stir and react for 30 minutes in an ice-water bath after the dropwise addition is completed, heating to room temperature after the reaction is completed, continuing the reaction for 48 hours, terminating the reaction, precipitating the prepared reactant in ice ether and stirring for 1 hour to obtain a crude product, filtering with ether three times and vacuum drying at 65°C for 12 hours to obtain a primary polymer;

[0013] In step S1, polyaspartic acid is first prepared, and then reacted with ethanolamine to connect the ethanolamine structure to the polyaspartic acid to prepare a primary polymer including the hydroxyl end of ethanolamine.

[0014] Step S3, adding N-methyldiallylamine into a four-necked flask, adding deionized water, stirring at a uniform speed, and then dropping a 10% by mass fraction dilute hydrochloric acid solution to adjust the pH until the pH is 7-8, then adding epichlorohydrin, heating to 40°C, stirring at a uniform speed and reacting for 6 hours, neutralizing with alkali after the reaction is completed, standing for 2 hours, separating the liquids, and removing the solvent by rotary evaporation to obtain a cationic monomer;

[0015] In step S3, N-methyldiallylamine and epichlorohydrin react to generate a cationic monomer, the structure of which is shown below:

[0016]

[0017] Step S4, adding the prepared cationic monomer to deionized water, stirring at a constant speed for 30 minutes, then adding the primary polymer, adding a 10% by mass sodium hydroxide solution, heating to 45-50° C., stirring at a constant speed and reacting for 6 hours to obtain a modified polyaspartic acid polymer.

[0018] In step S4, the cationic monomer reacts with the hydroxyl group on the primary polymer to undergo a covalent linking reaction, and then the primary polymer is grafted with a cationic modification to obtain a modified polyaspartic acid polymer; the modified polyaspartic acid polymer has the water solubility of polyaspartic acid itself, and contains amino groups in the molecule, which makes it easy to adhere to the rock surface through hydrogen bonds; on the other hand, the addition of amino acid polymers to water can increase the viscosity of the water phase, thereby reducing the chain growth ability of acrylamide during polymerization. In addition, after the primary polymer is modified, the introduction of cationic groups with positive charges can be adsorbed to the rock, thereby further improving the binding performance of the prepared modified polyaspartic acid polymer with the rock.

[0019] Further: in step S1, the amount ratio of L-aspartic acid and phosphoric acid is controlled to be 18-20mmol:10-12mmol, in step S2, the amount ratio of polyaspartic acid, N,N-dimethylformamide and ethanolamine is controlled to be 5-10g:25mL:1-1.2mL, in step S3, the amount ratio of N-methyldiallylamine, epichlorohydrin and deionized water is controlled to be 10mmol:10mmol:20mL, in step S4, the amount ratio of cationic monomer, primary polymer and deionized water is controlled to be 3-5g:5-8g:50mL, and the volume ratio of sodium hydroxide solution and deionized water is 1:10.

[0020] Furthermore, the N,N-dimethylformamide solution of ethanolamine in step S2 is prepared by mixing ethanolamine and N,N-dimethylformamide in a volume ratio of 1-1.2 mL: 2 mL.

[0021] A method for preparing a water-soluble temporary plugging agent for oil well fracturing comprises the following steps:

[0022] Acrylamide and modified polyaspartic acid polymer were added into deionized water, heated to 60°C, stirred at a uniform speed and reacted for 1 hour, then potassium persulfate was added, kept warm and reacted for 12 hours, filtered and dried after the reaction was completed, and a water-soluble temporary plugging agent for oil well fracturing was obtained.

[0023] Beneficial effects of the present invention:

[0024] The invention prepares a water-soluble temporary plugging agent for oil well fracturing. The water-swelling material is constructed by using polyacrylamide as the main material and a modified polyaspartic acid polymer. In the preparation process of the modified polyaspartic acid polymer, a covalent linking reaction is carried out between a synthesized cationic monomer and a hydroxyl group on a primary polymer, and then the primary polymer is grafted and cationized to obtain the modified polyaspartic acid polymer. The modified polyaspartic acid polymer has the water solubility of polyaspartic acid itself, and contains amino groups and the like in the molecule, so that it is easy to adhere to the rock surface through hydrogen bonds. On the other hand, after the amino acid polymer is added to water, the viscosity of the water phase can be increased, thereby reducing the chain growth ability of acrylamide during polymerization, thereby reducing the molecular weight of acrylamide during homopolymerization, and increasing the dissolution rate of the polymer in water. In addition, after the primary polymer is modified, a cationic group with a positive charge is introduced to be adsorbed to the rock, thereby further improving the binding performance of the prepared modified polyaspartic acid polymer with the rock, and improving the plugging ability of the temporary plugging agent. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1

[0027] The modified polyaspartic acid polymer comprises the following steps:

[0028] Step S1, adding L-aspartic acid and 85% by mass phosphoric acid into a three-necked flask, heating to 180° C. and reacting under reduced pressure for 2.5 h, then cooling to room temperature, dissolving with N,N-dimethylformamide and filtering, placing the filtrate in deionized water and stirring at a constant speed for 1 h, suction filtering, washing the filter cake with deionized water until the washing liquid is neutral, and then vacuum drying at 55° C. to obtain polyaspartic acid, wherein the amount ratio of L-aspartic acid to phosphoric acid is controlled to be 18 mmol: 10 mmol;

[0029] Step S2, adding the prepared polyaspartic acid to a three-necked flask filled with N,N-dimethylformamide, introducing nitrogen, magnetically stirring in an ice-water bath and slowly dropping a solution of ethanolamine in N,N-dimethylformamide, continuing to stir and react for 30 minutes in an ice-water bath after the addition is completed, heating to room temperature after the reaction is completed, continuing the reaction for 48 hours, terminating the reaction, precipitating the prepared reactant in ice ether and stirring for 1 hour to obtain a crude product, filtering with ether three times and vacuum drying at 65°C for 12 hours to obtain a primary polymer, and controlling the amount ratio of polyaspartic acid, N,N-dimethylformamide and ethanolamine to be 5g:25mL:1mL;

[0030] The N,N-dimethylformamide solution of ethanolamine is prepared by mixing ethanolamine and N,N-dimethylformamide in a volume ratio of 1 mL:2 mL.

[0031] Step S3, adding N-methyldiallylamine to a four-necked flask, adding deionized water, stirring at a uniform speed, and then dropping a 10% by mass fraction dilute hydrochloric acid solution to adjust the pH until the pH is 7-8, then adding epichlorohydrin, heating to 40°C, stirring at a uniform speed and reacting for 6 hours, neutralizing with alkali after the reaction is completed, standing for 2 hours, separating the liquids, and removing the solvent by rotary evaporation to obtain a cationic monomer, and controlling the amount ratio of N-methyldiallylamine, epichlorohydrin and deionized water to be 10mmol:10mmol:20mL;

[0032] Step S4, adding the prepared cationic monomer to deionized water, stirring at a uniform speed for 30 minutes, then adding the primary polymer, adding a 10% by mass sodium hydroxide solution, heating to 45°C, stirring at a uniform speed and reacting for 6 hours to obtain a modified polyaspartic acid polymer, controlling the dosage ratio of the cationic monomer, the primary polymer and deionized water to be 3g:5g:50mL, and the volume ratio of the sodium hydroxide solution to the deionized water to be 1:10.

[0033] Example 2

[0034] The modified polyaspartic acid polymer comprises the following steps:

[0035] Step S1, adding L-aspartic acid and 85% by mass phosphoric acid into a three-necked flask, heating to 180° C. and reacting under reduced pressure for 2.5 h, then cooling to room temperature, dissolving with N,N-dimethylformamide and filtering, placing the filtrate in deionized water and stirring at a constant speed for 1 h, suction filtering, washing the filter cake with deionized water until the washing liquid is neutral, and then vacuum drying at 55° C. to obtain polyaspartic acid, wherein the amount ratio of L-aspartic acid to phosphoric acid is controlled to be 19 mmol: 11 mmol;

[0036] Step S2, adding the prepared polyaspartic acid to a three-necked flask filled with N,N-dimethylformamide, introducing nitrogen, magnetically stirring in an ice-water bath and slowly dropping a solution of ethanolamine in N,N-dimethylformamide, continuing to stir and react for 30 minutes in an ice-water bath after the addition is completed, heating to room temperature after the reaction is completed, continuing the reaction for 48 hours, terminating the reaction, precipitating the prepared reactant in ice ether and stirring for 1 hour to obtain a crude product, filtering with ether three times and vacuum drying at 65°C for 12 hours to obtain a primary polymer, and controlling the amount ratio of polyaspartic acid, N,N-dimethylformamide and ethanolamine to be 8g:25mL:1.1mL;

[0037] The ethanolamine N,N-dimethylformamide solution is prepared by mixing ethanolamine and N,N-dimethylformamide in a volume ratio of 1-1.2 mL: 2 mL.

[0038] Step S3, adding N-methyldiallylamine to a four-necked flask, adding deionized water, stirring at a uniform speed, adding a 10% by mass fraction of dilute hydrochloric acid solution to adjust the pH until the pH is 7, then adding epichlorohydrin, heating to 40°C, stirring at a uniform speed and reacting for 6 hours, neutralizing with alkali after the reaction is completed, standing for 2 hours, separating the liquids, and removing the solvent by rotary evaporation to obtain a cationic monomer, and controlling the amount ratio of N-methyldiallylamine, epichlorohydrin and deionized water to be 10mmol:10mmol:20mL;

[0039] Step S4, adding the prepared cationic monomer to deionized water, stirring at a uniform speed for 30 minutes, then adding the primary polymer, adding a 10% by mass sodium hydroxide solution, heating to 48°C, stirring at a uniform speed and reacting for 6 hours to obtain a modified polyaspartic acid polymer, controlling the dosage ratio of the cationic monomer, the primary polymer and deionized water to be 4g:6g:50mL, and the volume ratio of the sodium hydroxide solution to the deionized water to be 1:10.

[0040] Example 3

[0041] The modified polyaspartic acid polymer comprises the following steps:

[0042] Step S1, adding L-aspartic acid and 85% by mass phosphoric acid into a three-necked flask, heating to 180° C. and reacting under reduced pressure for 2.5 h, then cooling to room temperature, dissolving with N,N-dimethylformamide and filtering, placing the filtrate in deionized water and stirring at a constant speed for 1 h, suction filtering, washing the filter cake with deionized water until the washing liquid is neutral, and then vacuum drying at 55° C. to obtain polyaspartic acid, wherein the amount ratio of L-aspartic acid to phosphoric acid is controlled to be 20 mmol: 12 mmol;

[0043] Step S2, adding the prepared polyaspartic acid to a three-necked flask filled with N,N-dimethylformamide, introducing nitrogen, magnetically stirring in an ice-water bath and slowly dropping a solution of ethanolamine in N,N-dimethylformamide, continuing to stir and react for 30 minutes in an ice-water bath after the dropwise addition is completed, heating to room temperature after the reaction is completed, continuing the reaction for 48 hours, terminating the reaction, precipitating the prepared reactant in ice ether and stirring for 1 hour to obtain a crude product, filtering with ether three times and vacuum drying at 65° C. for 12 hours to obtain a primary polymer, and controlling the amount ratio of polyaspartic acid, N,N-dimethylformamide and ethanolamine to be 10g:25mL:1.2mL;

[0044] The N,N-dimethylformamide solution of ethanolamine is prepared by mixing ethanolamine and N,N-dimethylformamide in a volume ratio of 1.2 mL:2 mL.

[0045] Step S3, adding N-methyldiallylamine to a four-necked flask, adding deionized water, stirring at a uniform speed, and then dropping a 10% by mass fraction dilute hydrochloric acid solution to adjust the pH until the pH is 8, then adding epichlorohydrin, heating to 40°C, stirring at a uniform speed and reacting for 6 hours, neutralizing with alkali after the reaction is completed, standing for 2 hours, separating the liquids, and removing the solvent by rotary evaporation to obtain a cationic monomer, and controlling the amount ratio of N-methyldiallylamine, epichlorohydrin and deionized water to be 10mmol:10mmol:20mL;

[0046] Step S4, adding the prepared cationic monomer to deionized water, stirring at a uniform speed for 30 minutes, then adding the primary polymer, adding a 10% by mass sodium hydroxide solution, heating to 50°C, stirring at a uniform speed and reacting for 6 hours to obtain a modified polyaspartic acid polymer, controlling the dosage ratio of the cationic monomer, the primary polymer and deionized water to be 5g:8g:50mL, and the volume ratio of the sodium hydroxide solution to the deionized water to be 1:10.

[0047] Example 4

[0048] A water-soluble temporary plugging agent for oil well fracturing, comprising the following raw materials in parts by weight: 20 parts of acrylamide, 15 parts of the modified polyaspartic acid polymer prepared in Example 1, 0.1 parts of potassium persulfate, and 50 parts of deionized water;

[0049] The water-soluble temporary plugging agent for oil well fracturing comprises the following steps:

[0050] Acrylamide and modified polyaspartic acid polymer were added into deionized water, heated to 60°C, stirred at a uniform speed and reacted for 1 hour, then potassium persulfate was added, kept warm and reacted for 12 hours, filtered and dried after the reaction was completed, and a water-soluble temporary plugging agent for oil well fracturing was obtained.

[0051] Example 5

[0052] A water-soluble temporary plugging agent for oil well fracturing, comprising the following raw materials in parts by weight: 25 parts of acrylamide, 20 parts of the modified polyaspartic acid polymer prepared in Example 2, 0.1 parts of potassium persulfate, and 60 parts of deionized water;

[0053] The water-soluble temporary plugging agent for oil well fracturing comprises the following steps:

[0054] Acrylamide and modified polyaspartic acid polymer were added into deionized water, heated to 60°C, stirred at a uniform speed and reacted for 1 hour, then potassium persulfate was added, kept warm and reacted for 12 hours, filtered and dried after the reaction was completed, and a water-soluble temporary plugging agent for oil well fracturing was obtained.

[0055] Example 6

[0056] A water-soluble temporary plugging agent for oil well fracturing, comprising the following raw materials in parts by weight: 30 parts of acrylamide, 25 parts of modified polyaspartic acid polymer prepared in an embodiment, 0.2 parts of potassium persulfate, and 70 parts of deionized water;

[0057] The water-soluble temporary plugging agent for oil well fracturing comprises the following steps:

[0058] Acrylamide and modified polyaspartic acid polymer were added into deionized water, heated to 60°C, stirred at a uniform speed and reacted for 1 hour, then potassium persulfate was added, kept warm and reacted for 12 hours, filtered and dried after the reaction was completed, and a water-soluble temporary plugging agent for oil well fracturing was obtained.

[0059] Comparative Example 1

[0060] Compared with Example 4, this comparative example uses the polyaspartic acid prepared in Example 1 to replace the modified polyaspartic acid polymer, and the preparation method is as follows:

[0061] Add acrylamide and polyaspartic acid into deionized water, heat to 60°C, stir uniformly and react for 1 hour, then add potassium persulfate, keep warm and react for 12 hours, filter and dry after the reaction to obtain a water-soluble temporary plugging agent for oil well fracturing.

[0062] Comparative Example 2

[0063] This comparative example is a water-soluble temporary plugging agent produced by a certain company on the market.

[0064] The performance of the water-soluble temporary plugging agents prepared in Examples 4-6 and Comparative Examples 1-2 was tested, and the results are shown in Table 1 below:

[0065] (1) Expansion rate: Calculate the expansion rate by immersing the prepared temporary plugging agent in 90℃ water for 1 hour and observing its volume change;

[0066] The calculation formula is as follows: (ΔV-ΔV 水 ) / V 暂堵剂 ;

[0067] ΔV refers to the total expansion volume during the expansion test, ΔV 水 is the expansion volume of water, V 暂堵剂 It refers to the volume of temporary plugging agent;

[0068] (2) Solubility: Dissolution time of temporary plugging agent in 90°C clean water, salt water, and 0.5% hydroxypropyl guar gum solution;

[0069] (3) Pressure bearing capacity and plugging rate: Place the temporary plugging agent sample into the core flow meter and simulate it through the instrument.

[0070] Table 1

[0071]

[0072] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A water-soluble temporary plugging agent for oil well fracturing, characterized in that: The method comprises the following raw materials in parts by weight: 20-30 parts of acrylamide, 15-25 parts of modified polyaspartic acid polymer, 0.1-0.2 parts of potassium persulfate, and 50-70 parts of deionized water; The water-soluble temporary plugging agent for oil well fracturing comprises the following steps: Add acrylamide and modified polyaspartic acid polymer into deionized water, heat to 60°C, stir uniformly and react for 1 hour, then add potassium persulfate, keep warm and react for 12 hours, filter and dry after the reaction, and obtain a water-soluble temporary plugging agent for oil well fracturing; The modified polyaspartic acid polymer comprises the following steps: Step S1, adding L-aspartic acid and 85% by mass phosphoric acid into a three-necked flask, heating to 180° C. and reacting under reduced pressure for 2.5 hours, then cooling to room temperature, dissolving with N,N-dimethylformamide and filtering, placing the filtrate in deionized water and stirring at a constant speed for 1 hour, suction filtering, washing the filter cake with deionized water until the washing liquid is neutral, and then vacuum drying at 55° C. to obtain polyaspartic acid; Step S2, adding the prepared polyaspartic acid into a three-necked flask filled with N,N-dimethylformamide, introducing nitrogen, magnetically stirring in an ice-water bath and slowly dropping a solution of ethanolamine in N,N-dimethylformamide, continuing to stir and react for 30 minutes in an ice-water bath after the dropwise addition is completed, heating to room temperature after the reaction is completed, continuing the reaction for 48 hours, terminating the reaction, precipitating the prepared reactant in ice ether and stirring for 1 hour to obtain a crude product, filtering with ether three times and vacuum drying at 65°C for 12 hours to obtain a primary polymer; Step S3, adding N-methyldiallylamine into a four-necked flask, adding deionized water, stirring at a uniform speed, and then dropping a 10% by mass fraction dilute hydrochloric acid solution to adjust the pH until the pH is 7-8, then adding epichlorohydrin, heating to 40°C, stirring at a uniform speed and reacting for 6 hours, neutralizing with alkali after the reaction is completed, standing for 2 hours, separating the liquids, and removing the solvent by rotary evaporation to obtain a cationic monomer; Step S4, adding the prepared cationic monomer to deionized water, stirring at a constant speed for 30 minutes, then adding the primary polymer, adding a 10% by mass sodium hydroxide solution, heating to 45-50° C., stirring at a constant speed and reacting for 6 hours to prepare a modified polyaspartic acid polymer; In step S1, the amount ratio of L-aspartic acid and phosphoric acid is controlled to be 18-20mmol: 10-12mmol, in step S2, the amount ratio of polyaspartic acid, N,N-dimethylformamide and ethanolamine is controlled to be 5-10g: 25mL: 1-1.2mL, in step S3, the amount ratio of N-methyldiallylamine, epichlorohydrin and deionized water is controlled to be 10mmol: 10mmol: 20mL, in step S4, the amount ratio of cationic monomer, primary polymer and deionized water is controlled to be 3-5g: 5-8g: 50mL, and the volume ratio of sodium hydroxide solution and deionized water is 1:

10.

2. The water-soluble temporary plugging agent for oil well fracturing according to claim 1, characterized in that: The N,N-dimethylformamide solution of ethanolamine in step S2 is prepared by mixing ethanolamine and N,N-dimethylformamide in a volume ratio of 1-1.2 mL: 2 mL.

3. The method for preparing a water-soluble temporary plugging agent for oil well fracturing according to claim 1, characterized in that: The steps include: Acrylamide and modified polyaspartic acid polymer were added into deionized water, heated to 60°C, stirred at a uniform speed and reacted for 1 hour, then potassium persulfate was added, kept warm and reacted for 12 hours, filtered and dried after the reaction was completed, and a water-soluble temporary plugging agent for oil well fracturing was obtained.