A resin silicon-carbon negative electrode material and preparation method thereof and lithium-ion battery

By forming a porous structure on the carbon source and using liquid resin impregnation and carbonization treatment, the carbon frame supports the silicon element is formed, and the problem of poor circulation performance of silicon carbon negative electrode materials is solved, the stability and capacity of the material are improved, and more efficient is achieved Lithium-ion battery performance.

CN117133899BActive Publication Date: 2024-12-03成都佰思格科技有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311173441.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-12
Publication Date
2024-12-03
Estimated Expiration
2043-09-12

AI Technical Summary

Technical Problem

The circulation performance of existing silicon-carbon negative electrode materials is poor, mainly due to the unstable structure of the silicon material during charging and discharging, which limits its application in lithium-ion batteries.

Method used

By performing porous treatment on the carbon source, the silicon source is introduced into the generated porous structure, and impregnated and carbonized with liquid resin to form a carbon frame to support the silicon element, reducing expansion and improving material structure stability.

Benefits of technology

It effectively alleviates the expansion problem of silicon-carbon anode material, improves its circulation performance and gram capacity, and enhances the unit volume utilization rate of the anode material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004444679950000101
    Figure BDA0004444679950000101
Patent Text Reader

Abstract

The present invention provides a resin silicon-carbon negative electrode material and a preparation method thereof and a lithium ion battery, and relates to the technical field of lithium ion batteries, wherein the preparation method comprises the following steps: mixing a silicon source, a foaming agent and a carbon source to obtain a mixture; heating the mixture to 200-250°C to obtain a hardened product; heating the hardened product to 710-900°C to obtain porous silicon-carbon; impregnating the porous silicon-carbon in a liquid resin to obtain impregnated silicon-carbon; heating the impregnated silicon-carbon to 710-900°C to obtain carbonized resin silicon-carbon; pulverizing the carbonized resin silicon-carbon to obtain a resin silicon-carbon negative electrode material. The present invention forms a porous structure on a carbon source by decomposing a foaming agent, so that the silicon element is embedded in the porous structure in situ, and the silicon element is supported by a carbon skeleton to relieve expansion; in combination with the impregnation step, the invalid pores generated by the foaming are effectively utilized to improve the stability of the negative electrode material structure and increase its gram capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a resin silicon-carbon negative electrode material and a preparation method thereof and a lithium ion battery. Background Art

[0002] Lithium-ion batteries have been widely used in various fields of daily life. As an important component of lithium-ion batteries, the performance of negative electrode materials directly determines the performance of lithium-ion batteries.

[0003] Currently, the commercial negative electrode materials are mainly graphite, but their theoretical capacity is relatively low; silicon materials have attracted widespread attention due to their higher theoretical capacity; however, due to the poor conductivity of silicon materials themselves and the large volume expansion during charging and discharging, the cycle performance is poor, which limits the application of silicon materials in lithium-ion battery negative electrode materials; to solve this problem, nano-silicon is currently usually used to prepare silicon-carbon composite materials, so as to improve the conductivity of the composite material while inhibiting the volume expansion of the material during charging and discharging to a certain extent, thereby improving its cycle performance.

[0004] Existing silicon-carbon negative electrode materials are usually prepared by directly mixing and sintering a silicon source and a carbon source. Although the silicon-carbon composite negative electrode material obtained by this preparation method has a certain improvement on the expansion of the silicon-carbon negative electrode material, the effect is not obvious and the cycle performance is poor. Summary of the invention

[0005] The technical problem to be solved by the present invention is: in order to solve the problem of poor cycle performance of silicon-carbon negative electrode materials in the prior art, the present invention provides a method for preparing a resin silicon-carbon negative electrode material. The preparation method introduces a silicon source into the generated porous structure during the process of making the carbon source porous, thereby enabling the prepared silicon-carbon negative electrode material to support silicon with a carbon skeleton, alleviate expansion, and improve the cycle performance of the silicon-carbon negative electrode material, thereby solving the problem of poor cycle performance of silicon-carbon negative electrode materials in the prior art.

[0006] The technical solution adopted by the present invention to solve its technical problem is:

[0007] A method for preparing a resin silicon-carbon negative electrode material comprises the following steps:

[0008] S1: mixing a silicon source, a foaming agent and a carbon source, and grinding them uniformly to obtain a mixture;

[0009] S2: heating the mixture to 200-250° C. and keeping the temperature for 8-12 hours to obtain a hardened product;

[0010] S3: heating the hardened product to 710-900° C., keeping the temperature for 3-8 hours, and cooling it to room temperature to obtain porous silicon carbon;

[0011] S4: impregnating the porous silicon carbon in a liquid resin for 1-5 hours to obtain impregnated silicon carbon;

[0012] S5: raising the temperature of the impregnated silicon carbon to 710-900° C. and keeping the temperature for 3-8 hours to obtain carbonized resin silicon carbon;

[0013] S6: crushing the carbonized resin silicon carbon to obtain a resin silicon carbon negative electrode material.

[0014] Optionally, the silicon source is nano-silicon.

[0015] Optionally, the foaming agent is sodium bicarbonate.

[0016] Optionally, the carbon source is selected from at least one of thermosetting resin, nitrocellulose, and cellulose acetate butyrate.

[0017] Optionally, the thermosetting resin is selected from at least one of phenolic resin, alkyd resin, amino resin, polyester resin, epoxy resin, polyurethane resin, acrylic resin, silicone resin, vinyl resin, fluororesin, polyketone resin, aldehyde resin, aldehyde-ketone resin, petroleum resin, terpene resin, polyester resin, chlorinated resin, furan resin, dammar resin, and maleic acid resin.

[0018] Optionally, the liquid resin in step S4 is liquid phenolic resin.

[0019] Optionally, in step S1, the mass ratio of the silicon source, the foaming agent and the carbon source is (5-15):1:90.

[0020] Another object of the present invention is to provide a resin silicon-carbon negative electrode material, which is prepared by the preparation method of the resin silicon-carbon negative electrode material as described above.

[0021] Another object of the present invention is to provide a lithium-ion battery comprising the resin silicon-carbon negative electrode material as described above.

[0022] The beneficial effects of the present invention are:

[0023] The preparation method of the resin silicon-carbon negative electrode material provided by the present invention, on the one hand, forms a porous structure on the carbon source through the decomposition of a foaming agent, and at the same time, the silicon element is embedded in the porous structure in situ, so that the silicon element is supported by the carbon skeleton to alleviate expansion; on the other hand, combined with the impregnation step, while improving the structural stability of the negative electrode material, the ineffective pores generated by foaming are effectively utilized, and while further suppressing expansion and improving the cycle performance of the negative electrode material, the stability of the negative electrode material structure is improved, and its gram capacity is increased, thereby indirectly improving the utilization rate per unit volume of the negative electrode material. DETAILED DESCRIPTION

[0024] The present invention is now further described in detail. The embodiments described below are exemplary and intended to be used to explain the present invention, but cannot be understood as limiting the present invention. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention belong to the scope of protection of the present invention.

[0025] In order to solve the problem of poor cycle performance of silicon-carbon negative electrode materials in the prior art, the present invention provides a method for preparing a resin silicon-carbon negative electrode material, which comprises the following steps:

[0026] S1: mixing a silicon source, a foaming agent and a carbon source, and grinding them evenly so that the silicon source and the foaming agent are evenly distributed in the carbon source to obtain a mixture;

[0027] S2: heating the mixture to 200-250°C and keeping the temperature for 8-12 hours to obtain a hardened product;

[0028] In this step, the carbon source in the mixture is hardened, and the foaming agent is partially decomposed; as the foaming agent decomposes, the carbon source adjacent to it collapses to generate a partial pore structure, and at the same time, the silicon source located near the pore structure enters the generated pore structure as the carbon source collapses. Therefore, in the hardened product obtained in this step, there is a partial pore structure on the carbon source, and part of the silicon source enters the pore structure;

[0029] S3: raising the temperature of the hardened product to 710-900°C, keeping the temperature for 3-8 hours, and cooling it to room temperature to obtain porous silicon carbon;

[0030] Through this step, the foaming agent is completely decomposed, and the gas generated by the foaming causes the carbon source to produce a porous structure. As the porous structure is produced, the silicon source located near the pore structure enters the porous structure, so that the carbon source acts as a carbon skeleton of silicon to support the silicon source, thereby achieving the purpose of alleviating expansion.

[0031] S4: impregnating the porous silicon carbon in a liquid resin for 1-5 hours to obtain impregnated silicon carbon;

[0032] By impregnating the material in the resin, on the one hand, it helps to further improve the stability of the material structure. On the other hand, since internal pores with an inner diameter of less than 1 nm are formed in the process of generating a porous structure through the decomposition of the foaming agent, these internal pores are too small to be embedded with the silicon source, making these pores invalid pores, thereby reducing the utilization rate of the unit volume of the negative electrode material. During the impregnation process, the resin enters these invalid pores to fill them, and the volume occupied by the invalid pores is utilized, which can improve the structural stability of the negative electrode material while improving its unit volume utilization rate.

[0033] S5: raising the temperature of the impregnated silicon carbon to 710-900°C and keeping the temperature for 3-8 hours to obtain carbonized resin silicon carbon;

[0034] This step completes the carbonization of the impregnated resin, so that the original ineffective pores are filled with carbon, and a carbon coating layer can be formed on the outer wall of the negative electrode material, thereby improving the structural stability and the unit volume utilization rate of the negative electrode material, and helping to increase the gram capacity of the negative electrode material;

[0035] S6: Crush the carbonized resin silicon carbon to obtain a resin silicon carbon negative electrode material.

[0036] The preparation method of the resin silicon-carbon negative electrode material provided by the present invention, on the one hand, forms a porous structure on the carbon source through the decomposition of a foaming agent, and at the same time, the silicon element is embedded in the porous structure in situ, so that the silicon element is supported by the carbon skeleton to alleviate expansion; on the other hand, combined with the impregnation step, while improving the structural stability of the negative electrode material, the ineffective pores generated by foaming are effectively utilized, and while further suppressing expansion and improving the cycle performance of the negative electrode material, the stability of the negative electrode material structure is improved, and its gram capacity is increased, thereby indirectly improving the utilization rate per unit volume of the negative electrode material.

[0037] In order to facilitate the smooth embedding of silicon elements into the porous structure during the foaming process, the preferred silicon source in the present invention is nano-silicon.

[0038] The preferred foaming agent of the present invention is sodium bicarbonate, the preferred carbon source is selected from at least one of thermosetting resin, nitrocellulose, and cellulose acetate butyrate, and the carbon source is further preferably a thermosetting resin, so that the resin silicon-carbon negative electrode material prepared in the present application is supported by the carbon skeleton of the resin, further improving the stability of the negative electrode material structure and improving its cycle performance.

[0039] Specifically, the preferred thermosetting resin of the present invention is selected from at least one of phenolic resin, alkyd resin, amino resin, polyester resin, epoxy resin, polyurethane resin, acrylic resin, silicone resin, vinyl resin, fluororesin, polyketone resin, aldehyde resin, aldehyde-ketone resin, petroleum resin, terpene resin, polyester resin, chlorinated resin, furan resin, dammar resin, and maleic acid resin.

[0040] To facilitate impregnation, the resin in step S4 is preferably a liquid resin; and when the impregnation resin selected is not liquid, it can be converted into a liquid state by heating or the like before impregnation.

[0041] Specifically, in the present invention, the liquid resin in step S4 is preferably a liquid phenolic resin.

[0042] In order to take into account both the electrochemical performance and the economy of the negative electrode material, the mass ratio of the silicon source, the foaming agent and the carbon source in step S1 of the present invention is preferably (5-15):1:90, and further preferably the mass ratio is 9:1:90.

[0043] Another object of the present invention is to provide a resin silicon-carbon negative electrode material, which is prepared by the method for preparing the resin silicon-carbon negative electrode material as described above.

[0044] The resin silicon-carbon negative electrode material provided by the present invention has the following advantages during its preparation: on the one hand, a porous structure is formed on a carbon source by decomposing a foaming agent, and silicon elements are embedded in the porous structure in situ, so that the silicon elements are supported by the carbon skeleton to alleviate expansion; on the other hand, in combination with the impregnation step, the structural stability of the negative electrode material is improved, and the ineffective pores generated by foaming are effectively utilized, so that the expansion is further suppressed, the cycle performance of the negative electrode material is improved, the structural stability of the negative electrode material is improved, and its gram capacity is increased, thereby indirectly improving the utilization rate per unit volume of the negative electrode material.

[0045] Another object of the present invention is to provide a lithium-ion battery comprising the resin silicon-carbon negative electrode material as described above.

[0046] In the preparation process of the negative electrode material selected for the lithium ion battery provided by the present invention, on the one hand, a porous structure is formed on a carbon source by decomposing a foaming agent, and silicon elements are embedded in the porous structure in situ, so that the silicon elements are supported by the carbon skeleton to alleviate expansion; on the other hand, in combination with the impregnation step, the structural stability of the negative electrode material is improved, and the ineffective pores generated by foaming are effectively utilized, so that the expansion is further suppressed, the cycle performance of the negative electrode material is improved, the structural stability of the negative electrode material is improved, and its gram capacity is increased, thereby indirectly improving the utilization rate of the unit volume of the negative electrode material.

[0047] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below.

[0048] Example 1

[0049] This embodiment provides a method for preparing a resin silicon-carbon negative electrode material, comprising the following steps:

[0050] S1: mixing nano silicon, sodium bicarbonate and phenolic resin in a mass percentage of 9:1:90 and grinding them evenly to obtain a mixture;

[0051] S2: heating the mixture to 220°C and keeping the temperature for 10 hours to obtain a hardened product;

[0052] S3: raising the temperature of the hardened product to 750°C and keeping the temperature for 5 hours to completely decompose the sodium bicarbonate therein, and the carbon dioxide gas generated by foaming makes the phenolic resin porous, and at the same time, the nano-silicon is embedded in the adjacent pore structure, and then the temperature is lowered to room temperature to obtain porous silicon carbon;

[0053] S4: Immersing the porous silicon carbon in liquid phenolic resin for 3 hours, allowing the resin to fill the remaining pores less than 1 nm, thereby obtaining impregnated silicon carbon;

[0054] S5: Continue to heat the impregnated silicon carbon in the tube furnace to 750°C and keep the temperature for 5 hours to complete the carbonization of the impregnated resin and obtain carbonized resin silicon carbon;

[0055] S6: Crush the carbonized resin silicon carbon to obtain a resin silicon carbon negative electrode material.

[0056] Example 2

[0057] This embodiment provides a method for preparing a resin silicon-carbon negative electrode material, comprising the following steps:

[0058] S1: mixing nano silicon, sodium bicarbonate and epoxy resin in a mass percentage of 9:1:90 and grinding them evenly to obtain a mixture;

[0059] S2: heating the mixture to 200°C and keeping the temperature for 10 hours to obtain a hardened product;

[0060] S3: raising the temperature of the hardened product to 750°C and keeping the temperature for 5 hours to completely decompose the sodium bicarbonate therein, and the carbon dioxide gas generated by foaming makes the epoxy resin porous, and at the same time, the nano-silicon is embedded in the adjacent pore structure, and then cooled to room temperature to obtain porous silicon carbon;

[0061] S4: Immersing the porous silicon carbon in liquid phenolic resin for 3 hours, allowing the resin to fill the remaining pores less than 1 nm, thereby obtaining impregnated silicon carbon;

[0062] S5: Continue to heat the impregnated silicon carbon in the tube furnace to 750°C and keep the temperature for 5 hours to complete the carbonization of the impregnated resin and obtain carbonized resin silicon carbon;

[0063] S6: Crush the carbonized resin silicon carbon to obtain a resin silicon carbon negative electrode material.

[0064] Example 3

[0065] This embodiment provides a method for preparing a resin silicon-carbon negative electrode material, comprising the following steps:

[0066] S1: mixing nano silicon, sodium bicarbonate and vinyl resin in a mass percentage of 9:1:90 and grinding them evenly to obtain a mixture;

[0067] S2: heating the mixture to 220°C and keeping the temperature for 10 hours to obtain a hardened product;

[0068] S3: raising the temperature of the hardened product to 750°C and keeping the temperature for 5 hours to completely decompose the sodium bicarbonate therein, and the carbon dioxide gas generated by foaming makes the vinyl resin porous, and at the same time, the nano-silicon is embedded in the adjacent pore structure, and then cooled to room temperature to obtain porous silicon carbon;

[0069] S4: Immersing the porous silicon carbon in liquid phenolic resin for 3 hours, allowing the resin to fill the remaining pores less than 1 nm, thereby obtaining impregnated silicon carbon;

[0070] S5: Continue to heat the impregnated silicon carbon in the tube furnace to 750°C and keep the temperature for 5 hours to complete the carbonization of the impregnated resin and obtain carbonized resin silicon carbon;

[0071] S6: Crush the carbonized resin silicon carbon to obtain a resin silicon carbon negative electrode material.

[0072] Comparative Example 1

[0073] This comparative example provides a method for preparing a negative electrode material, comprising the following steps:

[0074] S1: mixing nano silicon and phenolic resin in a mass percentage of 9:90 and grinding them evenly to obtain a mixture;

[0075] S2: heating the mixture to 220°C and keeping the temperature for 10 hours to obtain a hardened product;

[0076] S3: raising the temperature of the hardened product to 750°C and keeping the temperature for 5 hours to obtain silicon carbon;

[0077] S4: Crush the silicon carbon to obtain a negative electrode material.

[0078] Comparative Example 2

[0079] This comparative example provides a method for preparing a negative electrode material, comprising the following steps:

[0080] S1: mixing nano silicon, sodium bicarbonate and phenolic resin in a mass percentage of 9:1:90 and grinding them evenly to obtain a mixture;

[0081] S2: heating the mixture to 220°C and keeping the temperature for 10 hours to obtain a hardened product;

[0082] S3: raising the temperature of the hardened product to 750°C and keeping the temperature for 5 hours to completely decompose the sodium bicarbonate therein, and the carbon dioxide gas generated by foaming makes the phenolic resin porous, and at the same time, the nano-silicon is embedded in the adjacent pore structure, and then the temperature is lowered to room temperature to obtain porous silicon carbon;

[0083] S4: The porous silicon carbon is crushed to obtain a negative electrode material.

[0084] Comparative Example 3

[0085] This comparative example provides a method for preparing a negative electrode material, comprising the following steps:

[0086] S1: mixing sodium bicarbonate and phenolic resin in a mass percentage of 1:90 and grinding them evenly to obtain a mixture;

[0087] S2: heating the mixture to 220°C and keeping the temperature for 10 hours to obtain a hardened product;

[0088] S3: heating the hardened product to 750°C and keeping the temperature for 5 hours to completely decompose the sodium bicarbonate therein, and the carbon dioxide gas generated by foaming makes the phenolic resin porous, and then cooling it to room temperature to obtain a porous carbon material;

[0089] S4: mixing the nano-silicon and the porous carbon material in a mass ratio of 9:91 and grinding them evenly to obtain a silicon-carbon mixture;

[0090] S5: impregnating the silicon-carbon mixture in liquid phenolic resin for 3 hours, allowing the resin to fill the remaining pores less than 1 nm, thereby obtaining impregnated silicon-carbon;

[0091] S6: Continue to heat the impregnated silicon carbon in the tube furnace to 750° C. and keep the temperature for 5 hours to complete the carbonization of the impregnated resin and obtain carbonized resin silicon carbon;

[0092] S7: Crush the carbonized resin silicon carbon to obtain a negative electrode material.

[0093] Comparative Example 4

[0094] This comparative example provides a method for preparing a negative electrode material, comprising the following steps:

[0095] S1: mixing nano silicon, sodium bicarbonate and phenolic resin in a mass percentage of 9:1:90 and grinding them evenly to obtain a mixture;

[0096] S2: The mixture is heated to 750°C and kept at this temperature for 5 hours to completely decompose the sodium bicarbonate therein, and the carbon dioxide gas generated by foaming makes the phenolic resin porous, and at the same time, the nano-silicon is embedded in the adjacent pore structure, and then cooled to room temperature to obtain porous silicon carbon;

[0097] S3: Immersing the porous silicon carbon in liquid phenolic resin for 3 hours, allowing the resin to fill the remaining pores less than 1 nm, thereby obtaining impregnated silicon carbon;

[0098] S4: Continue to heat the impregnated silicon carbon in the tube furnace to 750°C and keep the temperature for 5 hours to complete the carbonization of the impregnated resin and obtain carbonized resin silicon carbon;

[0099] S5: crushing the carbonized resin silicon carbon to obtain a resin silicon carbon negative electrode material.

[0100] The negative electrode materials obtained in the above-mentioned embodiments and comparative examples are prepared into button-type batteries by a button-type battery process, and the preparation process is as follows: the materials prepared in the embodiments and comparative examples are respectively used as negative electrode active materials, and are evenly mixed with polyvinylidene fluoride (PVDF) (dissolved in N-methylpyrrolidone) and conductive carbon black in a mass ratio of 90:5:5, coated into an electrode film, placed in a vacuum drying oven at 120°C for 12 hours, and rolled and punched to obtain a hard carbon negative electrode plate; a metal lithium sheet is used as a counter electrode, 1 mol / LNaPF6 (EC-DEC=1:1) is used as an electrolyte, and the above-obtained negative electrode plates are assembled into 2430 button-type batteries in a glove box to test their electrochemical properties; and the negative electrode material is combined with a lithium iron phosphate positive electrode material to prepare a single cell, and a vernier caliper is used to detect the expansion rate of the single cell after 5 cycles; the test results are shown in Table 1.

[0101] Table 1

[0102]

[0103] It can be seen from the data in the above table that in the negative electrode materials prepared in Examples 1-3 of the present invention, the silicon element is effectively embedded in the resin carbon, and the pores in the resin carbon that are less than 1 nm are filled with the re-impregnated resin, and the gram capacity is relatively high; because the skeleton of the resin carbon ensures the rigidity of the silicon-carbon charge and discharge, the expansion rate of the single cell after 5 cycles changes by only 3%-5%, and the cycle performance is good.

[0104] In Comparative Example 1, the resin carbon was not made porous, the resin carbon did not form a skeleton, the silicon and the resin carbon were only mixed, and the resin carbon could not provide support for the silicon. Although its specific capacity was relatively high, its expansion rate changed significantly after 5 charge and discharge cycles, and its cycle performance was poor.

[0105] In Comparative Example 2, silicon is embedded in the skeleton of the resin carbon, but the pores of the resin carbon smaller than 1 nm are not filled later, resulting in a low specific capacity.

[0106] In Comparative Example 3, the resin carbon is first made porous, and then the porous resin carbon and nano-silicon are ground and mixed. Compared with Example 1, when sodium bicarbonate decomposes, that is, when the resin carbon produces pores, the nano-silicon cannot enter the pores when the pores are produced, and cannot be evenly distributed in the carbon pores, which will cause the nano-silicon to form a certain degree of aggregation. This aggregated part of the nano-silicon cannot be supported by the carbon skeleton, resulting in a high expansion rate and a low battery capacity retention rate; however, through the subsequent mixing of the nano-silicon with the porous carbon material, some of the nano-silicon can still enter the pores during the mixing process, so the capacity retention rate is slightly higher than that of Comparative Example 1.

[0107] Compared with Example 1, Comparative Example 4 reduces the step of heating and hardening the nano-silicon, sodium bicarbonate and phenolic resin, and directly heats to 750°C. Without the hardening process of the resin carbon, the structure formed after direct heating of the resin carbon will be unstable, and the carbon skeleton may even collapse. The silicon carbon cannot be protected by the collapsed carbon skeleton and cannot effectively inhibit the expansion. As a result, the battery expansion rate is high and the capacity retention rate is low.

[0108] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a resin silicon-carbon negative electrode material, characterized in that: The steps include: S1: mixing a silicon source, a foaming agent and a carbon source, and grinding them uniformly to obtain a mixture; S2: heating the mixture to 200-250° C. and keeping the temperature for 8-12 hours to obtain a hardened product; S3: heating the hardened product to 710-900° C., keeping the temperature for 3-8 hours, and cooling it to room temperature to obtain porous silicon carbon; S4: impregnating the porous silicon carbon in a liquid resin for 1-5 hours to obtain impregnated silicon carbon; S5: raising the temperature of the impregnated silicon carbon to 710-900° C. and keeping the temperature for 3-8 hours to obtain carbonized resin silicon carbon; S6: crushing the carbonized resin silicon carbon to obtain a resin silicon carbon negative electrode material; The silicon source is nano-silicon; The foaming agent is sodium bicarbonate; The carbon source is a thermosetting resin.

2. The method for preparing the resin silicon-carbon negative electrode material according to claim 1, characterized in that: The thermosetting resin is selected from at least one of phenolic resin, alkyd resin, amino resin, polyester resin, epoxy resin, polyurethane resin, acrylic resin, silicone resin, vinyl resin, fluororesin, polyketone resin, aldehyde resin, aldehyde-ketone resin, petroleum resin, terpene resin, polyester resin, chlorinated resin, furan resin, dammar resin, and maleic acid resin.

3. The method for preparing the resin silicon-carbon negative electrode material according to claim 1, characterized in that: The liquid resin in step S4 is liquid phenolic resin.

4. The method for preparing the resin silicon-carbon negative electrode material according to any one of claims 1 to 3, characterized in that: The mass ratio of the silicon source, the foaming agent and the carbon source in step S1 is (5-15): 1:

90.

5. A resin silicon-carbon negative electrode material, characterized in that: The method is used to prepare the resin silicon-carbon negative electrode material according to any one of claims 1 to 4.

6. A lithium ion battery, characterized in that: It includes the resin silicon-carbon negative electrode material as described in claim 5.