Combined inhibitor suitable for high-calcium-magnesium ilmenite and preparation method and application thereof

By using a combination inhibitor of carboxymethylcellulose sodium, sodium fluorosilicate and oxalic acid in high-calcium magnesium ilmenite flotation, the problem of poor separation of ilmenite and gangue minerals is solved, and high efficiency is achieved Titanium ore separation and recycling improves TiO2 grade and recovery, and reduces preparation and environmental costs.

CN117138969BActive Publication Date: 2024-11-01INST OF MULTIPURPOSE UTILIZATION OF MINERAL RESOURCES CHINESE ACAD OF GEOLOGICAL SCI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311298429.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-08
Publication Date
2024-11-01
Estimated Expiration
2043-10-08

AI Technical Summary

Technical Problem

The existing ilmenite flotation separation technology is difficult to effectively treat the relatively complex mineral composition of high calcium magnesium ilmenite, especially in the case of insufficient selectivity of gangue mineral inhibitors, which leads to ilmenite and gangue minerals. Poor separation effect.

Method used

Using a combination inhibitor, including sodium carboxymethylcellulose, sodium fluosilicate and oxalic acid, the flotation effect is significantly improved through synergistic action. The specific steps are: Sodium carboxymethylcellulose, sodium fluosilicate and oxalic acid. The specific proportions are mixed to form a solution and combined with collectors and other reagents during the flotation process to adjust the pH and temperature of the ore slurry to achieve selective separation of gangue minerals.

Benefits of technology

It significantly improves the grade and recovery of TiO2 in titanium ore, reduces the complexity of the dosage of the agent and the flotation process, ensures efficient ilmenite separation effect, and reduces the preparation cost and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117138969B_ABST
    Figure CN117138969B_ABST
Patent Text Reader

Abstract

The present disclosure relates to the technical field of beneficiation of high-calcium-magnesium ilmenite, and provides a combined inhibitor suitable for high-calcium-magnesium ilmenite, including sodium carboxymethyl cellulose, sodium fluorosilicate and oxalic acid. The present disclosure also provides a method for preparing the above-mentioned combined inhibitor, including: mixing sodium carboxymethyl cellulose with hot water and stirring, and adding sodium fluorosilicate and oxalic acid to obtain a mixed solution after the sodium carboxymethyl cellulose is completely dissolved; and stirring the mixed solution to obtain a combined inhibitor. The present disclosure also provides the use of the above-mentioned combined inhibitor in the flotation of high-calcium-magnesium ilmenite. The combined inhibitor provided by the present disclosure can at least effectively solve the problem of separation of gangue minerals in the flotation of high-calcium-magnesium ilmenite with relatively complex mineral composition, thereby improving the flotation effect, so as to achieve the effect of improving the grade and recovery rate of TiO2 in the obtained titanium ore.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of high-calcium-magnesium ilmenite beneficiation, and in particular to a combined inhibitor suitable for high-calcium-magnesium ilmenite, and a preparation method and application thereof. Background Art

[0002] Titanium metal has the characteristics of stable chemical properties, low density, high hardness, high temperature resistance, acid and alkali resistance and corrosion resistance, so it is widely used in aviation, military, transportation, environmental protection and medical industries. At present, flotation is still the main method for separating ilmenite. However, since the surface of gangue minerals (for example, silicate gangue minerals) contains not only the same Fe 3+ , Fe 2+ and Ti 4+ , and also contains Ca 2+ ,Mg 2+ and Al 3+ As the mine is mined to medium and deep depths, the ore gradually becomes poorer, finer, and more complex, and the Ca content in the minerals is 2+ and Mg 2+ The content of titanium is higher, so it is difficult to achieve flotation separation of ilmenite and gangue minerals using only collectors. In other words, it is difficult to obtain high-quality titanium concentrate products using traditional flotation reagent systems.

[0003] In this regard, existing studies have shown that it is difficult to simultaneously meet the selective separation of ilmenite and gangue minerals by collectors alone, and gangue mineral inhibitors need to be added to flotation to effectively improve the selectivity of collectors for ilmenite. Therefore, the development of highly selective gangue mineral inhibitors (e.g., silicate gangue mineral inhibitors) is an important way to improve the recovery efficiency of ilmenite. However, current research on the flotation separation of ilmenite is mainly based on collectors; compared with collectors, research on inhibitors in the flotation separation of ilmenite is relatively scarce, especially research on improving the selectivity of gangue mineral inhibitors.

[0004] At present, sulfuric acid, water glass and oxalic acid are commonly used silicate gangue mineral inhibitors in the flotation separation of ilmenite. Among them, sulfuric acid mainly dissolves the Ca on the surface of silicate gangue minerals. 2+ and Mg 2+ , preventing it from interacting with the collector, thereby inhibiting the floating of silicate gangue minerals; water glass mainly uses the negatively charged colloids produced by hydrolysis to adsorb to the surface of silicate gangue minerals, thereby inhibiting the floating of silicate gangue minerals, and studies have shown that water glass and the Mg on the surface of silicate gangue minerals 2+ There is a strong interaction; oxalic acid mainly interacts with the Ca 2+Calcium oxalate precipitates are formed to inhibit the floating of silicate gangue minerals. The silicate gangue mineral inhibitors commonly used in the flotation separation of the above-mentioned ilmenite have a certain sorting effect within a specific application range, and can better solve the separation problem of ilmenite and gangue minerals (for example, silicate gangue minerals) in ores with relatively simple mineral compositions; however, due to the insufficient selectivity of these silicate gangue mineral inhibitors, while inhibiting the floating of silicate gangue minerals, they will also strongly inhibit the floating of useful titanium-containing minerals. In view of this, for ores with relatively complex mineral compositions such as high-calcium-magnesium ilmenite, it is difficult to effectively solve the problems existing in the flotation of such ores if only the development of existing flotation reagent systems is considered.

[0005] In summary, there is an urgent need for an inhibitor to effectively solve the problems existing in the flotation of high-calcium-magnesium ilmenite with relatively complex mineral composition. Summary of the invention

[0006] The purpose of the present invention is to overcome the deficiency that the gangue mineral inhibitors (e.g., silicate gangue mineral inhibitors) in the prior art are difficult to effectively solve the problems existing in the flotation of high-calcium-magnesium ilmenite with relatively complex mineral composition due to insufficient selectivity, and to provide a combined inhibitor suitable for high-calcium-magnesium ilmenite and a preparation method and application thereof, so as to at least effectively solve the separation problem of gangue minerals (e.g., silicate gangue minerals) in the flotation of high-calcium-magnesium ilmenite with relatively complex mineral composition, improve the flotation effect, and thereby increase the TiO2 content in the obtained titanium ore. 2 The effect of grade and recovery rate.

[0007] The purpose of this disclosure is achieved through the following technical solutions:

[0008] In one aspect, a combined inhibitor applicable to high-calcium-magnesium ilmenite is provided, wherein the combined inhibitor comprises sodium carboxymethyl cellulose, sodium fluorosilicate and oxalic acid.

[0009] There is a synergistic effect between the sodium carboxymethyl cellulose, the sodium fluorosilicate and the oxalic acid in the combined inhibitor provided by the present disclosure, and the combined inhibitor has extremely strong selectivity; that is, under the condition that the dosage of the reagent remains unchanged, compared with the flotation effect achieved by using only one or two of the sodium carboxymethyl cellulose, the sodium fluorosilicate and the oxalic acid, the flotation effect achieved by the combined use of the sodium carboxymethyl cellulose, the sodium fluorosilicate and the oxalic acid can be significantly improved; therefore, the combined inhibitor can effectively solve the problem of separating gangue minerals (for example, silicate gangue minerals) in the flotation of the high-calcium-magnesium ilmenite with a relatively complex mineral composition. When the combined inhibitor is applied to the flotation of the high-calcium-magnesium ilmenite, the above-mentioned gangue minerals (for example, olivine and pyroxene) can be effectively inhibited, thereby achieving the improvement of the flotation effect under the conditions of a small dosage of the reagent and a simple flotation process, thereby significantly improving the TiO in the obtained titanium ore. 2 The effect of grade and recovery rate.

[0010] It is worth noting that the synergistic effect between the sodium carboxymethyl cellulose, the sodium fluorosilicate and the oxalic acid includes: the C 2 O 4 2- It can preferentially react with Ca in the above gangue minerals 2+ reacts with Fe in the gangue minerals mentioned above. 2+ and Mg 2+ The reaction causes the Ca on the surface of the gangue minerals to 2+ , Fe 2+ Mg 2+ The active sites are reduced, thereby preventing the collector from adsorbing the gangue minerals; on this basis, the sodium carboxymethyl cellulose can preferentially chemically adsorb on the surface of Mg in the pyroxene (e.g., titanium pyroxene) in the gangue minerals. 2+ The sodium fluorosilicate provides SiF 6 2- It can also be preferentially adsorbed on the surface of the above-mentioned titanium pyroxene to increase its hydrophilicity, thereby inhibiting the above-mentioned titanium pyroxene, and ultimately achieving the effect of further inhibiting the above-mentioned gangue minerals.

[0011] In some embodiments, the mass ratio of the sodium carboxymethyl cellulose, the sodium fluorosilicate and the oxalic acid is 2:5-7:1-3.

[0012] It should be noted that the ratio of the sodium carboxymethyl cellulose, the sodium fluorosilicate and the oxalic acid in the combined inhibitor depends on the content of the gangue minerals. When factors such as the properties of the original ore (for example, the type and content of the gangue minerals) change, the ratio of the sodium carboxymethyl cellulose, the sodium fluorosilicate and the oxalic acid can be adjusted accordingly to adapt to the changes.

[0013] In some examples, the mass ratio of the sodium carboxymethyl cellulose, the sodium fluorosilicate and the oxalic acid is 2:6:2; in this case, the combined inhibitor has better adaptability.

[0014] In another aspect, a method for preparing the combined inhibitor as described in any one of the above embodiments is provided, comprising: mixing and stirring the sodium carboxymethyl cellulose with hot water, and adding the sodium fluorosilicate and the oxalic acid to obtain a mixed solution after the sodium carboxymethyl cellulose is completely dissolved; and stirring the mixed solution to obtain the combined inhibitor.

[0015] In some embodiments, the stirring reaction temperature is 60-80° C., and the stirring reaction time is 1-3 h.

[0016] In some embodiments, the temperature of the hot water is 60-80°C.

[0017] In the above embodiment, by limiting the temperature of the hot water and the temperature of the stirring reaction, the dissolution and mixing of the components can be quickly and effectively promoted; on this basis, by further limiting the time of the stirring reaction, the time cost required for preparing the combined inhibitor can be reduced.

[0018] In yet another aspect, there is provided a use of the combined depressant as described in any one of the above embodiments in the flotation of high-calcium-magnesium ilmenite.

[0019] In some embodiments, the high-calcium-magnesium ilmenite includes gangue minerals, and the gangue minerals include olivine and pyroxene.

[0020] In some embodiments, the flotation comprises: adding the combined depressant and the complexing reagent to the slurry of the high-calcium-magnesium ilmenite to perform slurry mixing and flotation.

[0021] In the above embodiment, by using the combined depressant in combination with the complexing reagent, the selective separation of the gangue minerals in the flotation of the high-calcium-magnesium ilmenite can be achieved.

[0022] In some embodiments, the complexing agent includes at least one of a collector, a regulator, and diesel.

[0023] In some embodiments, the collector comprises MOH.

[0024] It should be noted that the MOH is a commonly used collector. According to the record in Chinese patent document CN201110165906.5, the MOH is composed of hydroxamic acid, styrene phosphoric acid, salicylic hydroxamic acid, oxidized paraffin soap and kerosene.

[0025] In some embodiments, the conditioning agent comprises sulfuric acid.

[0026] In some examples, the complexing reagent includes MOH, sulfuric acid, and diesel.

[0027] In the above example, by adopting the combined inhibitor, combining the MOH as the collector, and then using the sulfuric acid as the adjuster, the selective separation of the gangue minerals in the flotation of the high-calcium-magnesium ilmenite can be achieved, and there is no need to add other gangue mineral inhibitors during the slurry stirring and flotation.

[0028] In some embodiments, during the slurry mixing and flotation, the temperature of the slurry is 0-100°C.

[0029] In some embodiments, during the slurry mixing and flotation, the pH of the slurry is 2-5.

[0030] In the above embodiment, by limiting the pH of the slurry, the flotation effect of the combined depressant on the high-calcium-magnesium ilmenite can be ensured.

[0031] In some examples, during the slurry stirring and flotation, the pH of the slurry is 3-4; at this time, the combined depressant has a better flotation effect on the high-calcium-magnesium ilmenite.

[0032] In some embodiments, during the slurry stirring and flotation, the concentration of the combined depressant is less than or equal to 10 wt %.

[0033] It should be noted that the combined inhibitor disclosed in the present invention is not easy to dissolve, has strong viscosity and poor fluidity when the concentration is too high, and is not easy to add reagents during flotation; in view of this, diluting the combined inhibitor before adding can better control the dosage of the reagent, and the combined inhibitor can achieve a good flotation effect at a smaller dosage of the reagent.

[0034] In some examples, during the slurry stirring and flotation, the concentration of the combined depressant is 5 wt %.

[0035] It should be noted that the combined inhibitor has good fluidity when the concentration is below 10 wt %, and has better applicability when the concentration is 5 wt %.

[0036] The beneficial effects of the present disclosure are:

[0037] 1. The combined inhibitor for high-calcium-magnesium ilmenite disclosed in the present invention can effectively solve the separation problem of gangue minerals (e.g., silicate gangue minerals) in the flotation of high-calcium-magnesium ilmenite with relatively complex mineral composition. When the combined inhibitor is applied to the flotation of high-calcium-magnesium ilmenite, it can effectively inhibit gangue minerals (e.g., olivine and pyroxene), at least achieving the improvement of flotation effect under the conditions of small dosage of reagents and simple flotation process, thereby significantly improving the TiO2 content in the obtained titanium ore. 2 The effect of grade and recovery rate.

[0038] 2. The combined inhibitor disclosed in the present invention is suitable for high-calcium-magnesium ilmenite, which combines the advantages of each component and has a synergistic effect between the components, so that the combined inhibitor achieves an effect of 1+1+1 greater than 3 and has extremely strong selectivity.

[0039] 3. The combined inhibitor disclosed in the present invention is suitable for high-calcium-magnesium ilmenite, has a simple preparation process, low raw material cost, acid and alkali resistance, and is safe and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the technical solutions in the present disclosure, the following briefly introduces the drawings required to be used in some embodiments of the present disclosure. Obviously, the drawings described below are only drawings of some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can also be obtained based on these drawings. In addition, the drawings described below can be regarded as schematic diagrams, and are not limitations on the actual process of the method involved in the embodiments of the present disclosure.

[0041] Figure 1 A process flow chart of high calcium and magnesium ilmenite flotation provided by the present disclosure;

[0042] Figure 2 Another process flow chart of high-calcium-magnesium ilmenite flotation provided in the present disclosure. DETAILED DESCRIPTION

[0043] The technical solutions in some embodiments of the present disclosure are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments provided by the present disclosure, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present disclosure.

[0044] In the following, the terms "first" and "second" are used for descriptive purposes only and are not to be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features.

[0045] When describing some embodiments, the expression "A and / or B" may be used. It is easy to understand that "A and / or B" includes the following three combinations: only A, only B, and a combination of A and B.

[0046] When describing some embodiments, the expressions "at least one of A, B and C" and "at least one of A, B or C" may be used, both of which have the same meaning and include the following combinations of A, B and C: A only, B only, C only, the combination of A and B, the combination of A and C, the combination of B and C, and the combination of A, B and C.

[0047] Example 1

[0048] 1. A combined inhibitor suitable for high-calcium-magnesium ilmenite, comprising sodium carboxymethyl cellulose, sodium fluorosilicate and oxalic acid in a mass ratio of 2:6:2.

[0049] 2. A method for preparing the above-mentioned combined inhibitor, comprising:

[0050] S1. Place sodium carboxymethyl cellulose in a container, add hot water at 70°C and stir continuously until the sodium carboxymethyl cellulose is completely dissolved, add sodium fluorosilicate and oxalic acid to obtain a mixed solution;

[0051] S2. The mixed solution was stirred and reacted at 70°C for 2 hours to obtain the product.

[0052] Example 2

[0053] 1. A combined inhibitor suitable for high-calcium-magnesium ilmenite, comprising sodium carboxymethyl cellulose, sodium fluorosilicate and oxalic acid in a mass ratio of 2:5:3.

[0054] 2. A method for preparing the above-mentioned combined inhibitor, comprising:

[0055] S1. Place sodium carboxymethyl cellulose in a container, add hot water at 70°C and stir continuously until the sodium carboxymethyl cellulose is completely dissolved, add sodium fluorosilicate and oxalic acid to obtain a mixed solution;

[0056] S2. The mixed solution was stirred and reacted at 60°C for 2 h to obtain the product.

[0057] Example 3

[0058] 1. A combined inhibitor suitable for high-calcium-magnesium ilmenite, comprising sodium carboxymethyl cellulose, sodium fluorosilicate and oxalic acid in a mass ratio of 2:7:1.

[0059] 2. A method for preparing the above-mentioned combined inhibitor, comprising:

[0060] S1. Place sodium carboxymethyl cellulose in a container, add hot water at 70°C and stir continuously until the sodium carboxymethyl cellulose is completely dissolved, add sodium fluorosilicate and oxalic acid to obtain a mixed solution;

[0061] S2. The mixed solution was stirred and reacted at 80°C for 2 hours to obtain the product.

[0062] Example 4 Application of combined inhibitors

[0063] The combined depressant prepared in Example 1 was used for the flotation of high calcium and magnesium ilmenite in a certain factory and company in Panxi area. The test sample used in the flotation was the conventional coarse-grained flotation ore of high calcium and magnesium ilmenite. 2 The grade is 14.71%, the CaO grade is 10.17%, the MgO grade is 9.49%, and the SiO 2 The grade is 29.28%; it can be seen that the calcium and magnesium content in this test sample is relatively high.

[0064] Among them, the flotation process (such as Figure 1 As shown) includes S10~S40.

[0065] S10. Flotation desulfurization: adjust the pH of the floating material (i.e., the pulp of the conventional coarse-grained flotation ore) to a range of 5.5 to 6, and add sulfuric acid (H 2 SO 4 ), butyl xanthate and 2 # Oil, dosing interval is 3min, wait for 2 # After oil is added and stirred for 3 minutes, aeration flotation is performed to obtain sulfur concentrate and desulfurized tailings;

[0066] Among them, H 2 SO 4 The dosage is 500g / t, the dosage of butyl xanthate is 100g / t, 2 # The amount of oil used is 21g / t.

[0067] S20. Roughing: Adjust the pH of the desulfurized tailings slurry to approximately 3.5, and add H 2 SO 4 , combined inhibitor (YH-1), collector (MOH) and diesel, the dosing interval is 3 minutes, after adding diesel and stirring for 3 minutes, aeration flotation is carried out to obtain titanium rough concentrate and flotation tailings;

[0068] Among them, TiO 2 The grade is 25.31%, the grade of CaO is 7.31%, the grade of MgO is 7.56%, and the recovery rate is 80.13%; the TiO 2 The grade is 4.55%, and the recovery rate is 14.94%; 2 SO 4 The dosage is 2500g / t, the dosage of YH-1 is 400g / t, the dosage of MOH is 2500g / t, and the dosage of diesel is 150g / t.

[0069] S30. Sweep: Adjust the pH of the flotation tailings slurry to approximately 4, and add H 2 SO 4 and MOH, the dosing interval is 3min, after adding MOH and stirring for 3min, aeration flotation is carried out to obtain scavenged concentrate and tailings;

[0070] Among them, TiO 2 The grade is 4.38%, and the recovery rate is 21.41%; 2 SO 4 The dosage of is 200g / t, and the dosage of MOH is 200g / t.

[0071] S40. Selected I to Selected IV: Add H 2 SO 4 The pH of the initial slurry was adjusted to approximately 3, approximately 2.8, approximately 2.6 and approximately 2.5. 2 SO 4 Afterwards, the mixture was stirred for 3 minutes and aerated flotation was performed to finally obtain titanium concentrate;

[0072] Among them, TiO 2 The grade is 47.21%, the CaO grade is 1.17%, the MgO grade is 3.28%, and the recovery rate is 73.66%; 2 SO 4 The dosage is 400g / t, 300g / t, 200g / t and 200g / t respectively; the initial slurry of Selection I is the foam product of titanium rough concentrate (i.e., the slurry of titanium rough concentrate), the initial slurry of Selection II is the foam product obtained from Selection I, the initial slurry of Selection III is the foam product obtained from Selection II, and the initial slurry of Selection IV is the foam product obtained from Selection III.

[0073] Example 5 Application of combined inhibitors

[0074] The difference between Example 5 and Example 4 is that the combined inhibitor prepared in Example 1 is replaced by the combined inhibitor prepared in Example 2; other conditions such as the selection of remaining agents, agent dosage and process flow are the same as those of Example 4 of the present disclosure.

[0075] The results show that the TiO 2 The grade is 47.37%, the CaO grade is 0.87%, the MgO grade is 3.17%, and the recovery rate is 71.09%; the TiO 2 The grade is 4.84% and the recovery rate is 23.95%.

[0076] Example 6 Application of combined inhibitors

[0077] The difference between Example 6 and Example 4 is that the combined inhibitor prepared in Example 1 is replaced by the combined inhibitor prepared in Example 3; other conditions such as the selection of remaining agents, agent dosage and process flow are the same as those of Example 4 of the present disclosure.

[0078] The results show that the TiO 2 The grade is 47.08%, the CaO grade is 1.37%, the MgO grade is 3.20%, and the recovery rate is 74.31%; the TiO 2 The grade is 4.26% and the recovery rate is 20.76%.

[0079] Example 7 Application of combined inhibitors

[0080] The difference between Example 7 and Example 4 is that the dosage of the combined inhibitor in S20 is 200 g / t; other conditions such as the selection of reagents, the dosage of the remaining reagents and the process flow are the same as those of Example 4 of the present disclosure.

[0081] The results show that the TiO 2 The grade is 47.12%, the CaO grade is 1.33%, the MgO grade is 3.31%, and the recovery rate is 74.49%; the TiO 2 The grade is 4.23% and the recovery rate is 20.59%.

[0082] Example 8 Application of combined inhibitors

[0083] The difference between Example 8 and Example 4 is that the dosage of the combined inhibitor in S20 is 600 g / t; other conditions such as the selection of reagents, the dosage of the remaining reagents and the process flow are the same as those of Example 4 of the present disclosure.

[0084] The results show that the TiO 2The grade is 47.49%, the CaO grade is 0.83%, the MgO grade is 2.96%, and the recovery rate is 70.92%; the TiO 2 The grade is 4.87% and the recovery rate is 24.15%.

[0085] Comparative Example 1

[0086] The difference between Comparative Example 1 and Example 4 is that sodium fluorosilicate and oxalic acid are not added to the combined depressant, and the flotation process (such as Figure 2 other conditions such as the selection of the remaining reagents, the dosage of the reagents and the remaining process flow are the same as those of Example 4 of the present disclosure (compared with Example 4, this control example replaces the combined inhibitor comprising sodium carboxymethyl cellulose, sodium fluorosilicate and oxalic acid with an inhibitor comprising only sodium carboxymethyl cellulose under the condition that the dosage of the reagents remains unchanged, in order to prove that the combined inhibitor of the present disclosure is more effective).

[0087] The results show that the TiO 2 The grade is 28.75%, the CaO grade is 4.86%, the MgO grade is 4.35%, and the recovery rate is 61.17%; the TiO 2 The grade is 7.84% and the recovery rate is 33.91%.

[0088] Comparative Example 2

[0089] The difference between Comparative Example 2 and Example 4 is that sodium carboxymethyl cellulose and sodium fluorosilicate are not added to the combined depressant, and the flotation process (such as Figure 2 other conditions such as the selection of the remaining reagents, the dosage of the reagents and the remaining process flow are the same as those of Example 4 of the present disclosure (compared with Example 4, this control example replaces the combined inhibitor comprising sodium carboxymethyl cellulose, sodium fluorosilicate and oxalic acid with an inhibitor comprising only oxalic acid under the condition that the dosage of the reagents remains unchanged, in order to prove that the combined inhibitor of the present disclosure is more effective).

[0090] The results show that the TiO 2 The grade is 28.09%, the CaO grade is 4.23%, the MgO grade is 5.47%, and the recovery rate is 62.33%; the TiO 2 The grade is 7.74% and the recovery rate is 32.75%.

[0091] Comparative Example 3

[0092] The difference between the comparative example 3 and the example 4 is that sodium carboxymethyl cellulose and oxalic acid are not added to the combined inhibitor, and the flotation process (such as Figure 2other conditions such as the selection of the remaining reagents, the dosage of the reagents and the remaining process flow are the same as those of Example 4 of the present disclosure (compared with Example 4, this control example replaces the combined inhibitor comprising sodium carboxymethyl cellulose, sodium fluorosilicate and oxalic acid with an inhibitor comprising only sodium fluorosilicate under the condition that the dosage of the reagents remains unchanged, in order to prove that the combined inhibitor of the present disclosure is more effective).

[0093] The results show that the TiO 2 The grade is 23.53%, the grade of CaO is 9.62%, the grade of MgO is 10.21%, and the recovery rate is 81.15%; the TiO 2 The grade is 4.64% and the recovery rate is 13.93%.

[0094] Comparative Example 4

[0095] The difference between Comparative Example 4 and Example 4 is that the mass ratio of sodium carboxymethyl cellulose, sodium fluorosilicate and oxalic acid is 2:4:4, and the flotation process (such as Figure 2 Other conditions such as the selection of remaining reagents, the dosage of reagents and the remaining process flow are the same as those of Example 4 of the present disclosure (compared with Example 4, in this control example, under the condition that the dosage of reagents remains unchanged, the content of sodium fluorosilicate in the combined inhibitor is too low, while the content of oxalic acid is too high, which is used to prove that the combined inhibitor of the present disclosure is more effective).

[0096] The results show that the TiO 2 The grade is 25.19%, the CaO grade is 7.21%, the MgO grade is 7.49%, and the recovery rate is 76.81%; the TiO 2 The grade is 5.37% and the recovery rate is 18.27%.

[0097] Comparative Example 5

[0098] The difference between Comparative Example 5 and Example 4 is that the dosage of the combined depressant in S20 is 100 g / t, and the flotation process (such as Figure 2 Other conditions such as the selection of agents, the dosage of the remaining agents and the process flow are the same as those in Example 4 of the present disclosure (compared with Example 4, the dosage of the combined inhibitor in this control example is too low, which is used to prove that the combined inhibitor of the present disclosure has a better effect).

[0099] The results show that the TiO 2 The grade is 22.75%, the CaO grade is 8.94%, the MgO grade is 9.36%, and the recovery rate is 81.58%; the TiO 2 The grade is 4.71% and the recovery rate is 13.50%.

[0100] Comparative Example 6

[0101] The difference between Comparative Example 6 and Example 4 is that the dosage of the combined depressant in S20 is 700 g / t, and the flotation process (such as Figure 2 Other conditions such as the selection of agents, the dosage of the remaining agents and the process flow are the same as those in Example 4 of the present disclosure (compared with Example 4, the dosage of the combined inhibitor in this control example is too high, which is used to prove that the combined inhibitor of the present disclosure has a better effect).

[0102] The results show that the TiO 2 The grade is 25.87%, the CaO grade is 7.15%, the MgO grade is 7.38%, and the recovery rate is 78.98%; the TiO 2 The grade is 4.74% and the recovery rate is 16.10%.

[0103] Comparative Example 7

[0104] The difference between Comparative Example 7 and Example 4 is that no combined depressant is added in S20, and the flotation process (such as Figure 2 Other conditions such as the selection of remaining agents, the dosage of remaining agents and the remaining process flow are the same as those of Example 4 of the present disclosure (compared with Example 4, this control example does not add a combined inhibitor, which is used to prove that adding the combined inhibitor of the present disclosure has a better effect).

[0105] The results show that the TiO 2 The grade is 22.18%, CaO grade is 9.29%, MgO grade is 9.60%, and the recovery rate is 81.34%; the TiO 2 The grade is 4.94% and the recovery rate is 13.75%.

[0106] It should be noted that, for the flotation of high-calcium-magnesium ilmenite, the choice of flotation process will not affect the properties of the inhibitor itself. It can be seen that no matter what flotation process is used, the properties of the combined inhibitor provided by the present disclosure itself will not change, and it always has extremely strong selectivity, so it can achieve the selective separation of gangue minerals in the flotation of high-calcium-magnesium ilmenite. In addition, it can also be known that for the examples using different inhibitors, as long as the flotation processes used in these examples are exactly the same, then no matter what flotation process is used, these examples can achieve a comparison in the effect of the inhibitor. In other words, if these examples all use Figure 1 If the flotation process shown in the figure is used, then these examples can be compared in terms of the effect of the inhibitor; if these examples all use the flotation process shown in the figure, then these examples can be compared in terms of the effect of the inhibitor; Figure 2The flotation processes shown in FIG. 5A and FIG. 5B , then these examples also enable a comparison of the effects of the inhibitors.

[0107] On this basis, in order to reduce the steps required for comparison, the present disclosure adopts the following method in comparative examples 1 to 7: Figure 2 The flotation process shown in Figure 2 The flotation process shown is similar to Figure 1 The flotation processes shown differ only in that Figure 2 The flotation process shown does not include S30-S40; on this basis, by comparing the titanium rough concentrate and flotation tailings obtained in S20 of Example 4 with the titanium rough concentrate and flotation tailings obtained in S20 of Comparative Examples 1-7, it can be regarded that Example 4 compared with Comparative Examples 1-7 also adopts Figure 2 In the flotation process shown, at this time, the comparison between Example 4 and Comparative Examples 1 to 7 in terms of the inhibitor effect can be achieved.

[0108] Experimental results

[0109] The products obtained in each step of Examples 4 to 8 and Comparative Examples 1 to 7 were dried, weighed and sent for testing to obtain the yield, TiO 2 The grade and recovery rate of ore, the grade and recovery rate of CaO and the grade and recovery rate of MgO.

[0110] The results are shown in Tables 1 and 2:

[0111] Table 1

[0112]

[0113]

[0114] Table 2

[0115]

[0116]

[0117] According to the records in Tables 1 and 2 above, we can at least know that:

[0118] 1. When the combined depressant disclosed in the present invention is applied to the flotation of high calcium and magnesium ilmenite, it can effectively inhibit gangue minerals, thereby improving the flotation effect under the conditions of small dosage of reagents and simple flotation process, and at least achieving the purpose of increasing the yield of the obtained titanium ore (titanium rough concentrate or titanium concentrate) and the TiO 2 The effect of reducing the grade and recovery rate of CaO and the grade and recovery rate of MgO in the obtained titanium ore (titanium rough concentrate or titanium concentrate);

[0119] 2. Compared with the control example 7, the yield of titanium crude concentrate in the control example 1 was significantly reduced, and TiO 2 The grade of titanium concentrate increased slightly, the recovery rate decreased significantly, the grades of CaO and MgO decreased slightly, and the recovery rates of CaO and MgO decreased significantly; the yield of titanium concentrate in Comparative Example 2 decreased significantly, TiO 2 The grade of CaO and MgO slightly increased, the recovery rate decreased significantly, the grade of CaO and MgO slightly decreased, and the recovery rate of CaO and MgO decreased significantly; the yield of titanium crude concentrate in Comparative Example 3 decreased slightly, TiO 2 The grade of titanium concentrate in Example 4 increased slightly, the recovery rate did not change significantly, the grades of CaO and MgO increased slightly, and the recovery rate of CaO decreased slightly; the yield of titanium concentrate in Example 4 decreased slightly, TiO 2 The grade of CaO increased slightly, the recovery rate did not change significantly, the grades of CaO and MgO decreased slightly, and the recovery rates of CaO and MgO decreased significantly;

[0120] Compared with Example 4, the yield of titanium crude concentrate in Comparative Example 1 was significantly reduced, and TiO 2 The grade of titanium concentrate increased slightly, and the recovery rate decreased significantly; the yield of titanium concentrate in Comparative Example 2 decreased significantly, and TiO 2 The grade of titanium concentrate increased slightly, and the recovery rate decreased significantly; the yield of titanium concentrate in Comparative Example 3 increased slightly, and the recovery rate of TiO 2 The grade of CaO decreased slightly, and the recovery rate increased slightly, while the grades of CaO and MgO increased significantly, and the recovery rates of CaO and MgO increased significantly;

[0121] It can be seen that compared with no addition of inhibitors, the addition of the inhibitors used in Control Examples 1 to 3 and the combined inhibitors used in Example 4 can improve the flotation effect. However, Example 4 can at least simultaneously improve the TiO 2 That is to say, under the condition that the dosage of the reagent remains unchanged, the flotation effect achieved by the combined inhibitor used in Example 4 is significantly better than that achieved by the inhibitors used in Control Examples 1 to 3, which indicates that the flotation effect achieved by the combined use of sodium carboxymethyl cellulose, sodium fluorosilicate and oxalic acid is better than the flotation effect achieved by using only one of sodium carboxymethyl cellulose, sodium fluorosilicate and oxalic acid, so the components in the combined inhibitor disclosed in the present invention have a synergistic effect.

[0122] Therefore, the combined inhibitor for high-calcium-magnesium ilmenite disclosed in the present invention, as well as its preparation method and application, can effectively solve the problem of separating gangue minerals in the flotation of high-calcium-magnesium ilmenite with relatively complex mineral composition. When the combined inhibitor is applied to the flotation of high-calcium-magnesium ilmenite, the gangue minerals can be effectively inhibited, at least achieving the goal of improving the flotation effect under the conditions of small dosage of reagents and simple flotation process, thereby significantly improving the TiO in the obtained titanium ore. 2 The effect of grade and recovery rate.

[0123] The above is only a preferred embodiment of the present disclosure. It should be understood that the present disclosure is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not deviate from the spirit and scope of the present disclosure, and should be within the scope of protection of the claims attached to the present disclosure.

Claims

1. A combined inhibitor suitable for high calcium and magnesium ilmenite, characterized in that: Includes sodium carboxymethylcellulose, sodium fluorosilicate, and oxalic acid; The mass ratio of the sodium carboxymethyl cellulose, the sodium fluorosilicate and the oxalic acid is 2:5-7:1-3.

2. A method for preparing the combined inhibitor according to claim 1, characterized in that: include: The sodium carboxymethyl cellulose is mixed with hot water and stirred, and after the sodium carboxymethyl cellulose is completely dissolved, the sodium fluorosilicate and the oxalic acid are added to obtain a mixed solution; and The mixed solution is stirred for reaction to obtain the combined inhibitor.

3. The method according to claim 2, characterized in that The stirring reaction temperature is 60 to 80° C., and the stirring reaction time is 1 to 3 hours; And / or, the temperature of the hot water is 60-80°C.

4. Use of the combined depressant as claimed in claim 1 in the flotation of high calcium and magnesium ilmenite.

5. The use according to claim 4, characterized in that: The high-calcium-magnesium ilmenite includes gangue minerals, and the gangue minerals include olivine and pyroxene.

6. The use according to claim 5, characterized in that: The flotation comprises: The combined depressant and the complexing agent are added into the slurry of the high-calcium-magnesium ilmenite for slurry mixing and flotation.

7. The use according to claim 6, characterized in that: The complexing agent includes at least one of a collector, a regulator and diesel.

8. The use according to claim 7, characterized in that: The collector comprises MOH; And / or, the conditioning agent comprises sulfuric acid.

9. The use according to claim 6, characterized in that: During the slurry mixing and flotation, the temperature of the slurry is 0 to 100°C; And / or, during the slurry mixing and flotation, the pH of the slurry is 2 to 5; And / or, during the slurry stirring and flotation, the concentration of the combined depressant is less than or equal to 10 wt %.

Citation Information

Patent Citations

  • Medicament for mineral separation and floatation of ilmenite in Shandong province

    CN102294305A

  • Mineral processing method of titanium-containing molten and separated slag

    CN102921552A

  • Combined inhibitor for olivine flotation and prepration method and application of combined inhibitor

    CN109604068A

  • Silicate gangue mineral inhibitor for flotation of Ti-containing mineral and application of inhibitor

    CN110076005A

  • Dispersion inhibitor suitable for ultra-fine particle ilmenite as well as preparation method and application of dispersion inhibitor

    CN112871460A