Polyfunctional naphthalene compound and preparation method, curing agent, resin composition and adhesive
By developing the polyfunctional naphthalene compound 1,5-bis(3-mercaptopropoxy)-2,6-bis(3-mercaptopropyl)naphthalene, the problem of existing polythiol curing agents in high temperature and hot and humid environments has been solved. Heat resistance and odor issues, the polyfunctional naphthalene compound that is liquid at room temperature has good heat resistance and moisture-heat resistance, and is suitable for adhesives and resin compositions of electronic materials.
Patent Information
- Application Number
- CN202311105870.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-08-30
AI Technical Summary
Existing polythiol curing agents have insufficient heat resistance in high temperature and hot and humid environments, poor heat and humidity resistance, short pot life and unpleasant odor, and cannot meet the stringent requirements of electronic materials for adhesives.
Develop a polyfunctional naphthalene compound with the structure of 1,5-bis(3-mercaptopropoxy)-2,6-bis(3-mercaptopropyl)naphthalene, which is liquid at room temperature through a specific preparation method, It has good heat resistance, moisture and heat resistance and low odor, and can be directly used as a curing agent for curing resin compositions.
It is realized that the polyfunctional naphthalene compound that is liquid at room temperature has good heat resistance, moisture and heat resistance and long pot life, and has low odor. It can improve the storage stability of one-component low-temperature curing epoxy resin and has a long pot life. Adhesives and resin compositions suitable for electronic materials.
Smart Images

Figure CN117142992B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of curing agents and their application, and in particular to a polyfunctional naphthalene compound and a preparation method thereof, a curing agent, a resin composition and an adhesive. Background Art
[0002] With the continuous development of the mobile network era, electronic equipment is gradually developing towards the trend of being light and thin, and high-power, and the requirements for electronic materials and electronic packaging materials are also constantly increasing. Epoxy resin, as one of the most important polymer packaging matrix materials, has high bonding performance, low dielectric constant and excellent electrical insulation performance, and has become the most important basic resin material in electronic packaging materials. In order to protect semiconductor components to make the circuit highly centralized or improve the connection reliability, adhesives and sealing materials containing epoxy resin compositions are often used. In particular, in the case of semiconductor devices containing components that deteriorate under high temperature conditions, their manufacturing processes all need to be carried out under low temperature conditions. In addition, in the assembly and assembly of electronic components, for the purpose of maintaining reliability, no matter what material the bonded substrate is made of, it is often necessary to use adhesives and sealants with high reliability of moisture-resistant bonding strength. Furthermore, it is also required to enable the resin composition to be used for a long time, that is, a long application period.
[0003] Epoxy resin and epoxy curing agent together construct the three-dimensional structure of thermosetting materials, so the curing agent largely determines the final performance of thermosetting materials. Different epoxy resin curing agents have different chemical structures and reactivity, so the choice of curing agent depends on the process technology, material application period, curing conditions and the final requirements for material performance. Polythiol curing agents are often used in epoxy adhesives to achieve the combined effect of low-temperature rapid curing and storage stability. However, the most commonly used commercial thiol curing agents in the past are trifunctional and tetrafunctional thiols (such as PETMP, TMPMP, etc.) and secondary polythiols (such as PE1, etc.), which have insufficient heat resistance after curing with epoxy resin, and very poor resistance to moisture and heat, especially in a humid and hot environment. The bulk strength and bonding strength of the material will decay rapidly, making it difficult to meet the stringent requirements of electronic materials, and there is a strong odor problem, which seriously affects the working environment during gluing.
[0004] Therefore, there is an urgent need to develop an epoxy resin curing agent compound that is liquid at room temperature and has good heat resistance, moisture and heat resistance, long-term applicability and low odor to meet the increasingly stringent demands in the development of electronic materials. Summary of the invention
[0005] The purpose of the present invention is to provide a polyfunctional naphthalene compound and a preparation method, a curing agent, a resin composition and an adhesive, which overcome the defects of the existing polythiol curing agent, such as insufficient heat resistance, poor moisture and heat resistance, long applicable period and bad odor. The polyfunctional naphthalene compound of the present invention is liquid at room temperature and can simultaneously have good heat resistance, moisture and heat resistance, long applicable period and low odor.
[0006] To achieve the above object, the technical solution adopted by the present invention is: a polyfunctional naphthalene compound, the structural formula of the polyfunctional naphthalene compound is:
[0007]
[0008] Among them, R 1 , R 2 , R 3 and R 4 C 1-5 The alkylene group includes, but is not limited to, methylene, ethylene, n-propylene, isopropylene, n-butylene, sec-butylene, isobutylene, tert-butylene, n-pentylene, isopentylene, tert-pentylene or neopentylene.
[0009] As a further optimization, R 1 and R 3 R is n-propylene, 2 and R 4 C 2-5 of alkylene.
[0010] The present invention also provides a method for preparing a polyfunctional naphthalene compound, comprising the following steps:
[0011] Step 1: dissolving dihydroxynaphthalene in a mixed solvent of acetone and N,N-dimethylformamide, adding a base and a catalyst, heating to 30-80°C under nitrogen protection and stirring for 5-30 minutes, then adding a halogenated compound, reacting for 2-8 hours, filtering and removing the solvent under reduced pressure, washing with water and drying, and then heating to 150-250°C and reacting for 2-4 hours to obtain a first intermediate product;
[0012] Step 2: dissolving the first intermediate product in a mixed solvent of acetone and N,N-dimethylformamide, adding a base and a catalyst, heating to 30-80°C under nitrogen protection and stirring for 5-30 minutes, then adding a halogenated compound, reacting for 2-8 hours, filtering and removing the solvent under reduced pressure, washing with water and drying to obtain a second intermediate product;
[0013] Step 3: dissolve the second intermediate product and thioacetic acid in tetrahydrofuran, add a photoinitiator, stir and react under ultraviolet light for 20-40 minutes, evaporate the solvent and the remaining thioacetic acid under reduced pressure, dissolve it again with tetrahydrofuran, then add a methanol solution of hydrochloric acid or sodium hydroxide, heat to 20-80°C and react for 2-8 hours, evaporate the solvent under reduced pressure, wash with water and dry to obtain a colorless or light yellow liquid polyfunctional naphthalene compound.
[0014] As a further optimization, the halogenated compound in step 1 and step 2 is a straight-chain or branched alkane with one end of the molecular chain capped with chlorine or bromine and the other end capped with a double bond.
[0015] As a further optimization, the base in step one and step two includes one or a combination of potassium carbonate, sodium carbonate, sodium hydroxide, potassium hydroxide, triethylamine and p-dimethylaminopyridine; the catalyst includes one or a combination of alkylammonium chlorides, sodium alkyl sulfonates, chain polyethers, cyclic crown ethers, and cyclodextrin catalysts.
[0016] As a further optimization, the photoinitiator in step one is a free radical photoinitiator; the free radical photoinitiator is a cleavage-type photoinitiator and / or a hydrogen abstraction-type photoinitiator.
[0017] The present invention also provides a curing agent, which at least comprises the above-mentioned multi-functional naphthalene compound.
[0018] The present invention also provides a resin composition, which comprises at least a resin and the above-mentioned curing agent, wherein the resin comprises one or a combination of benzaldehyde compounds, epoxy resins, olefins or acrylate compounds having carbon-carbon double bonds in the molecules.
[0019] As a further optimization, the resin composition also includes a curing accelerator. When the resin is a benzaldehyde compound, the curing accelerator is trifluoroacetic acid; when the resin is an epoxy resin, the curing accelerator is an amine; when the resin is an olefin or acrylate compound having a carbon-carbon double bond in the molecule, the curing accelerator is a free radical photoinitiator.
[0020] The present invention also provides an adhesive, which at least comprises the above-mentioned resin composition.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The polyfunctional naphthalene compound of the present invention has good heat resistance, good resistance to moisture and heat, and low odor;
[0023] 2. The polyfunctional naphthalene compound of the present invention is liquid at room temperature and can be directly used as a curing agent for curing the resin composition without the need for additional coupling to form an oligomer mixture or for use in combination with other polythiol compounds. The cost is low, and the resin composition prepared using the curing agent containing the polyfunctional naphthalene compound can be used as a component of an adhesive;
[0024] 3. The polyfunctional naphthalene compound of the present invention can improve the storage stability of the single-component low-temperature curing epoxy resin, has a long applicable period, and has broad application prospects. DETAILED DESCRIPTION
[0025] The following are specific embodiments of the present invention, which further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments.
[0026] Example 1
[0027] This example is used to illustrate the preparation of the polyfunctional naphthalene compound 1,5-bis(3-mercaptopropoxy)-2,6-bis(3-mercaptopropyl)naphthalene provided by the present invention. The specific steps are as follows:
[0028] Step 1: dissolving 80 g of dihydroxynaphthalene in a mixed solvent of 150 mL of acetone and 50 mL of N,N-dimethylformamide, adding 93.6 g of potassium carbonate and 8.05 g of tetrabutylammonium bromide, heating to 60 ° C and stirring for 20 minutes under nitrogen protection, then adding 75 g of allyl bromide, continuing to react for 6 hours, filtering and removing the solvent under reduced pressure, washing with water and drying, and then heating to 200 ° C for 3 hours to obtain a first intermediate product;
[0029] Step 2: dissolve the first intermediate product in a mixed solvent of 150 mL acetone and 50 mL N,N-dimethylformamide, add 103.6 g potassium carbonate and 8.3 g tetrabutylammonium bromide, heat to 60 ° C and stir for 20 minutes under nitrogen protection, then add 79 g allyl bromide, react for 6 hours, filter and evaporate the solvent under reduced pressure, wash with water and dry to obtain a second intermediate product;
[0030] Step 3: Mix the second intermediate product and 90g of thioacetic acid, dissolve in 200mL of tetrahydrofuran, add 2.1g of 2,2'-dimethoxy-2-phenylacetophenone, stir and react under ultraviolet light for 30 minutes, evaporate the solvent and the remaining thioacetic acid under reduced pressure, dissolve again with 200mL of tetrahydrofuran, then add 30mL of 1mol / L hydrochloric acid methanol solution, heat to 50°C and react for 8 hours, evaporate the solvent under reduced pressure, wash with water and dry to obtain 200.8g of a colorless or light yellow liquid product, which is a multi-official naphthalene compound 1,5-bis(3-mercaptopropoxy)-2,6-bis(3-mercaptopropyl)naphthalene, with a total yield of 88.4%, and the multi-official naphthalene compound has substantially no sulfur odor.
[0031] Example 2
[0032] This example is used to illustrate the preparation of the polyfunctional naphthalene compound 1,5-bis(4-mercaptobutyloxy)-2,6-bis(3-mercaptopropyl)naphthalene provided by the present invention. The specific steps are as follows:
[0033] Step 1: dissolve 80 g of dihydroxynaphthalene in a mixed solvent of 100 mL of acetone and 50 mL of N,N-dimethylformamide, add 90 g of potassium carbonate and 6.7 g of tetrabutylammonium bromide, heat to 30 ° C and stir for 5 minutes under nitrogen protection, then add 70 g of 4-bromo-1-butene, continue to react for 2 hours, filter and evaporate the solvent under reduced pressure, wash with water and dry, and then heat to 150 ° C and react for 2 hours to obtain a first intermediate product;
[0034] Step 2: dissolve the first intermediate product in a mixed solvent of 100 mL acetone and 50 mL N, N-dimethylformamide, add 100 g potassium carbonate and 7.9 g tetrabutylammonium bromide, heat to 30 ° C and stir for 5 minutes under nitrogen protection, then add 75 g 4-bromo-1-butene, react for 2 hours, filter and evaporate the solvent under reduced pressure, wash with water and dry to obtain a second intermediate product;
[0035] Step 3: Mix the second intermediate product and 90g of thioacetic acid, dissolve in 150mL of tetrahydrofuran, add 1.5g of methyl benzoylformate, stir and react under ultraviolet light for 20 minutes, remove the solvent and the remaining thioacetic acid under reduced pressure, dissolve again with 150mL of tetrahydrofuran, then add 25mL of 1mol / L methanol solution of hydrochloric acid, warm to 20°C and react for 4 hours, remove the solvent under reduced pressure, wash with water and dry to obtain 200.9g of a colorless or light yellow liquid product, which is a multi-official naphthalene compound 1,5-bis(3-mercaptopropoxy)-2,6-bis(3-mercaptopropyl)naphthalene, with a total yield of 83%, and the multi-official naphthalene compound has substantially no sulfur odor.
[0036] Example 3
[0037] This example is used to illustrate the preparation of the polyfunctional naphthalene compound (1,5-bis(5-mercaptopentyloxy)-2,6-bis(3-mercaptopropyl)naphthalene) provided by the present invention. The specific steps are as follows:
[0038] Step 1: dissolving 80 g of dihydroxynaphthalene in a mixed solvent of 200 mL of acetone and 50 mL of N,N-dimethylformamide, adding 105 g of potassium carbonate and 9.5 g of tetrabutylammonium bromide, heating to 80 ° C and stirring for 30 minutes under nitrogen protection, then adding 80 g of 5-bromo-1-pentene, continuing to react for 8 hours, filtering and removing the solvent under reduced pressure, washing with water and drying, and then heating to 250 ° C for 4 hours to obtain a first intermediate product;
[0039] Step 2: dissolve the first intermediate product in a mixed solvent of 200 mL acetone and 50 mL N, N-dimethylformamide, add 108 g potassium carbonate and 8.3 g tetrabutylammonium bromide, heat to 80 ° C and stir for 30 minutes under nitrogen protection, then add 85 g 5-bromo-1-pentene, react for 8 hours, filter and evaporate the solvent under reduced pressure, wash with water and dry to obtain a second intermediate product;
[0040] Step 3: Mix the second intermediate product and 95g of thioacetic acid, dissolve in 250mL of tetrahydrofuran, add 3g of 2-hydroxy-2-methyl-phenylacetone-1, stir and react under ultraviolet light for 40 minutes, evaporate the solvent and the remaining thioacetic acid under reduced pressure, dissolve again with 250mL of tetrahydrofuran, then add 55mL of 1mol / L methanol solution of sodium hydroxide, heat to 80°C and react for 12 hours, evaporate the solvent under reduced pressure, wash with water and dry to obtain 222.6g of a colorless or light yellow liquid product, which is a multi-official naphthalene compound 1,5-bis(5-mercaptopentyloxy)-2,6-bis(3-mercaptopropyl)naphthalene, with a total yield of 86.9%. The multi-official naphthalene compound has substantially no sulfur odor.
[0041] Example 4
[0042] This embodiment is used to illustrate the preparation of the thermosetting resin composition provided by the present invention. The resin composition comprises the following components in parts by weight: component A comprises 60 parts of 4-hydroxy-3-methoxybenzaldehyde, 30 parts of styrenated phenol, 2 parts of fumed silica, and 0.5 parts of carbon black; component B comprises 90 parts of the multi-functional naphthalene compound 1,5-bis(3-mercaptopropoxy)-2,6-bis(3-mercaptopropyl)naphthalene prepared in Example 1, 5 parts of trifluoroacetic acid, and 2 parts of fumed silica, ensuring that the ratio of thiol to aldehyde functional groups is 2.
[0043] After measuring the above raw materials in a container, the A and B components are fully mixed at room temperature or low temperature using a dispersing device, and degassing treatment is performed. The discharged materials are packaged in a double tube to obtain a resin composition.
[0044] Example 5
[0045] This embodiment is used to illustrate the preparation of the thermosetting resin composition provided by the present invention. The resin composition comprises the following components in parts by weight: component A comprises 60 parts of 4-hydroxy-3-methoxybenzaldehyde, 30 parts of styrenated phenol, 2 parts of fumed silica, and 0.5 parts of carbon black; component B comprises 95 parts of the multi-functional naphthalene compound 1,5-bis(4-mercaptobutyloxy)-2,6-bis(3-mercaptopropyl)naphthalene prepared in Example 2, 5 parts of trifluoroacetic acid, and 2 parts of fumed silica, ensuring that the ratio of thiol to aldehyde functional groups is 2.
[0046] After measuring the above raw materials in a container, the A and B components are fully mixed at room temperature or low temperature using a dispersing device, and degassing treatment is performed. The discharged materials are packaged in a double tube to obtain a resin composition.
[0047] Example 6
[0048] This embodiment is used to illustrate the preparation of the thermosetting resin composition provided by the present invention. The resin composition comprises the following components in parts by weight: component A comprises 60 parts of 4-hydroxy-3-methoxybenzaldehyde, 30 parts of styrenated phenol, 2 parts of fumed silica, and 0.5 parts of carbon black; component B comprises 100 parts of the multi-functional naphthalene compound 1,5-bis(5-mercaptopentyloxy)-2,6-bis(3-mercaptopropyl)naphthalene prepared in Example 3, 5 parts of trifluoroacetic acid, and 2 parts of fumed silica, ensuring that the ratio of thiol to aldehyde functional groups is 2.
[0049] After measuring the above raw materials in a container, the A and B components are fully mixed at room temperature or low temperature using a dispersing device, and degassing treatment is performed. The discharged materials are packaged in a double tube to obtain a resin composition.
[0050] Example 7
[0051] This embodiment is used to illustrate the preparation of the one-component epoxy resin composition provided by the present invention. The resin composition comprises the following components in parts by weight: 50 parts of bisphenol A epoxy resin, 10 parts of hydrogenated bisphenol A epoxy resin, 36 parts of the multi-official naphthalene compound 1,5-bis(3-mercaptopropoxy)-2,6-bis(3-mercaptopropyl)naphthalene prepared in Example 1, 3 parts of a latent curing accelerator, 0.5 parts of a stabilizer triethyl borate, and 2 parts of fumed silica.
[0052] After measuring the above raw materials in a container, use a dispersing device to fully mix them at room temperature or low temperature, and perform a degassing treatment. After discharging and packaging, the resin composition is obtained.
[0053] Example 8
[0054] This example is used to illustrate the preparation of the one-component epoxy resin composition provided by the present invention. The resin composition includes the following components in parts by weight: 50 parts of bisphenol A epoxy resin, 10 parts of hydrogenated bisphenol A epoxy resin, 38 parts of the multi-official naphthalene compound 1,5-bis(4-mercaptobutyloxy)-2,6-bis(3-mercaptopropyl)naphthalene prepared in Example 2, 3 parts of a latent curing accelerator, 0.5 parts of a stabilizer triethyl borate, and 2 parts of fumed silica.
[0055] After measuring the above raw materials in a container, use a dispersing device to fully mix them at room temperature or low temperature, and perform a degassing treatment. After discharging and packaging, the resin composition is obtained.
[0056] Example 9
[0057] This example is used to illustrate the preparation of the one-component epoxy resin composition provided by the present invention. The resin composition comprises the following components in parts by weight: 50 parts of bisphenol A epoxy resin, 10 parts of hydrogenated bisphenol A epoxy resin, 40 parts of the multi-official naphthalene compound 1,5-bis(5-mercaptopentyloxy)-2,6-bis(3-mercaptopropyl)naphthalene prepared in Example 3, 3 parts of latent curing accelerator, 0.5 parts of stabilizer triethyl borate, and 2 parts of fumed silica.
[0058] After measuring the above raw materials in a container, use a dispersing device to fully mix them at room temperature or low temperature, and perform a degassing treatment. After discharging and packaging, the resin composition is obtained.
[0059] Example 10
[0060] This example is used to illustrate the preparation of the UV light-curable resin composition provided by the present invention. The resin composition comprises the following components in parts by weight: 50 parts of bisphenol A epoxy diacrylate, 10 parts of tricyclodecane dimethanol diacrylate, 30 parts of the multi-official naphthalene compound 1,5-bis(3-mercaptopropoxy)-2,6-bis(3-mercaptopropyl)naphthalene prepared in Example 1, 3 parts of a photoinitiator 2,2-dimethoxy-2-phenylacetophenone, and 0.2 parts of a polymerization inhibitor p-hydroxyanisole.
[0061] After measuring the above raw materials in a container, use a dispersing device to fully mix them at room temperature or low temperature in a dark environment, and perform a degassing treatment. After discharging and packaging, the resin composition is obtained.
[0062] Embodiment 11
[0063] This example is used to illustrate the preparation of the UV light-curable resin composition provided by the present invention. The resin composition comprises the following components in parts by weight: 50 parts of bisphenol A epoxy diacrylate, 10 parts of tricyclodecane dimethanol diacrylate, 32 parts of 1,5-bis(4-mercaptobutyloxy)-2,6-bis(3-mercaptopropyl)naphthalene prepared in Example 2, 3 parts of photoinitiator 2,2-dimethoxy-2-phenylacetophenone, and 0.2 parts of inhibitor p-hydroxyanisole.
[0064] After measuring the above raw materials in a container, use a dispersing device to fully mix them at room temperature or low temperature in a dark environment, and perform a degassing treatment. After discharging and packaging, the resin composition is obtained.
[0065] Example 12
[0066] This example is used to illustrate the preparation of the UV light-curable resin composition provided by the present invention. The resin composition comprises the following components in parts by weight: 50 parts of bisphenol A epoxy diacrylate, 10 parts of tricyclodecane dimethanol diacrylate, 34 parts of the multi-official naphthalene compound 1,5-bis(4-mercaptopentyloxy)-2,6-bis(3-mercaptopropyl)naphthalene prepared in Example 3, 3 parts of a photoinitiator 2,2-dimethoxy-2-phenylacetophenone, and 0.2 parts of a polymerization inhibitor p-hydroxyanisole.
[0067] After measuring the above raw materials in a container, use a dispersing device to fully mix them at room temperature or low temperature in a dark environment, and perform a degassing treatment. After discharging and packaging, the resin composition is obtained.
[0068] Example 13
[0069] This example is used to illustrate the preparation of the light / heat dual-curing resin composition provided by the present invention. The resin composition includes the following components in parts by weight: 25 parts of bisphenol A epoxy resin, 5 parts of hydrogenated bisphenol A epoxy resin, 25 parts of bisphenol A epoxy diacrylate, 5 parts of tricyclodecane dimethanol diacrylate, 33 parts of the multi-official naphthalene compound 1,5-bis(3-mercaptopropoxy)-2,6-bis(3-mercaptopropyl)naphthalene prepared in Example 1, 1 part of photoinitiator 2-hydroxy-2-methyl-1-phenylacetone and 1 part of diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide, 2 parts of latent curing accelerator, 0.3 parts of stabilizer triethyl borate, and 0.1 parts of inhibitor p-hydroxyanisole.
[0070] After measuring the above raw materials in a container, use a dispersing device to fully mix them at room temperature or low temperature in a dark environment, and perform a degassing treatment. After discharging and packaging, the resin composition is obtained.
[0071] Embodiment 14
[0072] This example is used to illustrate the preparation of the light / heat dual-curing resin composition provided by the present invention. The resin composition includes the following components in parts by weight: 25 parts of bisphenol A epoxy resin, 5 parts of hydrogenated bisphenol A epoxy resin, 25 parts of bisphenol A epoxy diacrylate, 5 parts of tricyclodecane dimethanol diacrylate, 35 parts of the multi-official naphthalene compound 1,5-bis(4-mercaptobutyloxy)-2,6-bis(3-mercaptopropyl)naphthalene prepared in Example 2, 1 part of photoinitiator 2-hydroxy-2-methyl-1-phenylacetone and 1 part of diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide, 2 parts of latent curing accelerator, 0.3 parts of stabilizer triethyl borate, and 0.1 parts of inhibitor p-hydroxyanisole.
[0073] After taking the above raw materials into a container, use a dispersing device to fully mix them at room temperature or low temperature in a dark environment, and perform a degassing treatment. After discharging and packaging, the resin composition is obtained.
[0074] Embodiment 15
[0075] This example is used to illustrate the preparation of the light / heat dual-curing resin composition provided by the present invention. The resin composition includes the following components in parts by weight: 25 parts of bisphenol A epoxy resin, 5 parts of hydrogenated bisphenol A epoxy resin, 25 parts of bisphenol A epoxy diacrylate, 5 parts of tricyclodecane dimethanol diacrylate, 37 parts of the multi-official naphthalene compound 1,5-bis(5-mercaptopentyloxy)-2,6-bis(3-mercaptopropyl)naphthalene prepared in Example 3, 1 part of photoinitiator 2-hydroxy-2-methyl-1-phenylacetone and 1 part of diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide, 2 parts of latent curing accelerator, 0.3 parts of stabilizer triethyl borate, and 0.1 parts of inhibitor p-hydroxyanisole.
[0076] After measuring the above raw materials in a container, use a dispersing device to fully mix them at room temperature or low temperature in a dark environment, and perform a degassing treatment. After discharging and packaging, the resin composition is obtained.
[0077] In the above embodiments, the latent curing accelerator is from Ajinomoto Fine Chemicals Co., Ltd. and its brand name is AJICURE PN-23.
[0078] Comparative Example 1
[0079] A thermosetting resin composition was prepared according to the method of Example 4, except that the polyfunctional naphthalene compound 1,5-bis(3-mercaptopropoxy)-2,6-bis(3-mercaptopropyl)naphthalene in Example 4 was replaced by a polythiol curing agent pentaerythritol tetrakis(3-mercaptopropionic acid)ester with the same thiol functional group equivalent, and the other conditions were the same as in Example 4 to obtain a thermosetting resin composition.
[0080] Comparative Example 2
[0081] A one-component epoxy resin composition was prepared according to the method of Example 7, except that the polyfunctional naphthalene compound 1,5-bis(3-mercaptopropoxy)-2,6-bis(3-mercaptopropyl)naphthalene in Example 4 was replaced by a polythiol curing agent pentaerythritol tetrakis(3-mercaptopropionic acid)ester with the same thiol functional group equivalent, and the other conditions were the same as in Example 7 to obtain a one-component epoxy resin composition.
[0082] Comparative Example 3
[0083] A UV-curable resin composition was prepared according to the method of Example 10, except that the polyfunctional naphthalene compound 1,5-bis(3-mercaptopropoxy)-2,6-bis(3-mercaptopropyl)naphthalene in Example 10 was replaced by a polythiol curing agent pentaerythritol tetrakis(3-mercaptopropionic acid)ester with the same thiol functional group equivalent, and the other conditions were the same as in Example 10 to obtain a UV-curable resin composition.
[0084] Comparative Example 4
[0085] A light / heat dual-cure resin composition was prepared according to the method of Example 13, except that the polyfunctional naphthalene compound 1,5-bis(3-mercaptopropoxy)-2,6-bis(3-mercaptopropyl)naphthalene in Example 13 was replaced by a polythiol curing agent pentaerythritol tetrakis(3-mercaptopropionic acid)ester with the same thiol functional group equivalent, and the other conditions were the same as in Example 13 to obtain a light / heat dual-cure resin composition.
[0086] Test Case
[0087] (1) Curing conditions: The resin compositions prepared in Examples 4-6 and Comparative Example 1 were squeezed out of double-tube packaging using a dispensing machine, mixed in a static mixer, and then cured at room temperature for 60 minutes to obtain cured samples; the resin compositions prepared in Examples 7-9 and Comparative Example 2 were placed in an oven at 80° C. for thermal curing for 60 minutes to obtain cured samples; the resin compositions prepared in Examples 10-12 and Comparative Example 3 were placed in an oven at 80° C. for thermal curing for 60 minutes to obtain cured samples; the resin compositions prepared in Examples 10-12 and Comparative Example 3 were placed in an oven at 80° C. for thermal curing for 60 minutes to obtain cured samples. 2 ) for 10 seconds to obtain a cured sample; the resin compositions prepared in Examples 13-15 and Comparative Example 4 were first irradiated with an ultraviolet light source (365 nm, light intensity 1000 mW / cm 2 ) for 4 seconds, and then the sample was placed in an oven at 80°C for thermal curing for 60 minutes to obtain a cured sample.
[0088] (2) Glass transition temperature (°C): The test was conducted using a Q-800 dynamic mechanical analysis tester (DMA) from TA Instruments, USA. The resin compositions prepared in the above embodiments and comparative examples were completely cured to form thin sheets of 42 mm×8 mm×0.3 mm. The variation of the loss factor (tan δ) with temperature was measured in a liquid nitrogen atmosphere and film stretching mode within a temperature range of -40 to 250°C. The heating rate was 10°C / min and the test frequency was 10 Hz, so as to determine the glass transition temperature T of the cured resin composition. g (℃).
[0089] (3) Bond strength (MPa): The resin compositions prepared in the above embodiments and comparative examples were coated on stainless steel sheets, overlapped and pressed with tempered glass sheets to make test samples with a bonding area of 25.4 mm×5 mm and a thickness of the adhesive layer of 0.1 mm. The test samples were cured, and then the two sheets of the completely cured samples were pulled apart in opposite directions using a universal testing machine. The samples were tested at ambient temperatures of 25°C and 90°C, respectively, and the measured force values were recorded as strength (MPa). The cured samples were subjected to heating and humidification conditions of 85°C / 85% RH / 168 h, and the shear bond strength (MPa) of the samples was tested again at an ambient temperature of 90°C and recorded.
[0090] The measurement results of the glass transition temperature and the thermal adhesive strength before and after heating and humidification are shown in the following table.
[0091]
[0092] By analyzing and comparing Examples 4-15 and / or Comparative Examples 1-4 through experimental data analysis, firstly, by analyzing Examples 1-3, it can be seen that the poly-official naphthalene compound of the present invention is in liquid state, has a high yield, and basically no by-products are produced, the preparation process is simple, and the cost can be effectively reduced; by comparing and analyzing Example 4 and Comparative Example 1, Example 7 and Comparative Example 2, Example 10 and Comparative Example 3, Example 13 and Comparative Example 4, it can be seen that the resin composition prepared by using the poly-official naphthalene compound of the present invention as a curing agent is significantly better in terms of glass transition temperature and thermal bonding strength before and after heating and humidification, indicating that the resin composition prepared by the present invention has higher heat resistance (high glass transition temperature and high thermal bonding strength), better bonding performance and moisture and heat resistance.
[0093] From the comparison of Example 4, Example 7, Example 10, and Example 15 with Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4, it can be seen that after the polyfunctional naphthalene compound prepared by the present invention is replaced with the commercial polythiol curing agent pentaerythritol tetrakis(3-mercaptopropionic acid), the glass transition temperature of the resin composition after curing is sharply reduced, and the thermal bonding strength is also significantly reduced, especially the thermal bonding strength after heating and humidification almost disappears, indicating that the polyfunctional naphthalene compound of the present invention has a significant effect on the heat resistance, bonding performance and moisture-heat hydrolysis resistance of the resin composition.
[0094] Based on the above analysis, the polyfunctional naphthalene compound of the present invention has low odor, no ester bond, good heat resistance and moisture-heat resistance, is liquid at room temperature, and can be directly used as a curing agent for the preparation of a resin composition, which can be used as a component of an adhesive. In addition, the polythiol compound provided by the present invention can reduce the storage stability risk of a single-component low-temperature curing epoxy resin, has a long applicable period, and has broad application prospects.
[0095] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.
Claims
1. Polyfunctional naphthalene compounds, It is characterized in that The structural formula of the polyofficial naphthalene compound is: Among them, R 1 , R 2 , R 3 and R 4 C 1-5 of alkylene; The preparation method of the polyofficial naphthalene compound comprises the following steps: Step 1: dissolving dihydroxynaphthalene in a mixed solvent of acetone and N,N-dimethylformamide, adding a base and a catalyst, heating to 30-80°C under nitrogen protection and stirring for 5-30 minutes, then adding a halogenated compound, reacting for 2-8 hours, filtering and removing the solvent under reduced pressure, washing with water and drying, and then heating to 150-250°C and reacting for 2-4 hours to obtain a first intermediate product; Step 2: dissolving the first intermediate product in a mixed solvent of acetone and N,N-dimethylformamide, adding a base and a catalyst, heating to 30-80°C under nitrogen protection and stirring for 5-30 minutes, then adding a halogenated compound, reacting for 2-8 hours, filtering and removing the solvent under reduced pressure, washing with water and drying to obtain a second intermediate product; Step 3: dissolving the second intermediate product and thioacetic acid in tetrahydrofuran, adding a photoinitiator, stirring and reacting under ultraviolet light for 20-40 minutes, distilling off the solvent and the remaining thioacetic acid under reduced pressure, dissolving again in tetrahydrofuran, then adding a methanol solution of hydrochloric acid or sodium hydroxide, heating to 20-80° C. and reacting for 2-8 hours, distilling off the solvent under reduced pressure, washing with water and drying to obtain a colorless or light yellow liquid polyfunctional naphthalene compound; The halogenated compound in step 1 and step 2 is a straight-chain or branched alkane with one end of the molecular chain capped by chlorine or bromine and the other end capped by a double bond.
2. The polyfunctional naphthalene compound according to claim 1, It is characterized in that R 1 and R 3 R is n-propylene, 2 and R 4 C 2-5 of alkylene.
3. The polyfunctional naphthalene compound according to claim 1, It is characterized in that The base in step one and step two includes one or a combination of potassium carbonate, sodium carbonate, sodium hydroxide, potassium hydroxide, triethylamine and p-dimethylaminopyridine; the catalyst includes one or a combination of alkylammonium chlorides, alkyl sodium sulfonates, chain polyethers, cyclic crown ethers and cyclodextrin catalysts.
4. The polyfunctional naphthalene compound according to claim 1, It is characterized in that The photoinitiator in step three is a free radical photoinitiator; the free radical photoinitiator is a cleavage-type photoinitiator and / or a hydrogen abstraction-type photoinitiator.
5. Curing agent, It is characterized in that The curing agent comprises at least the polyfunctional naphthalene compound according to any one of claims 1 to 4.
6. Resin composition, It is characterized in that The resin composition at least comprises a resin and the curing agent according to claim 5, wherein the resin comprises one or a combination of benzaldehyde compounds, epoxy resins, olefins or acrylate compounds having carbon-carbon double bonds in the molecules.
7. The resin composition according to claim 6, It is characterized in that The resin composition also includes a curing accelerator. When the resin is a benzaldehyde compound, the curing accelerator is trifluoroacetic acid; when the resin is an epoxy resin, the curing accelerator is an amine; when the resin is an olefin or acrylate compound having a carbon-carbon double bond in the molecule, the curing accelerator is a free radical photoinitiator.
8. Adhesives, It is characterized in that The adhesive comprises at least the resin composition according to claim 6 or 7.