A composite wave absorbing material, electromagnetic shielding film and preparation method thereof
CoFe2O4 nanosheets were prepared by hydrothermal method and loaded with TiO2 nanoparticles. Combined with polyaniline coating, the problem of high reflection loss of electromagnetic shielding materials in the prior art is solved, and a composite wave absorbing material with high shielding efficiency and low reflection loss is achieved. Suitable for electronic devices.
Patent Information
- Application Number
- CN202311009189.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-11
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-08-11
AI Technical Summary
In the prior art, when preparing electromagnetic shielding materials, it is difficult to achieve high shielding efficiency and low reflection loss at the same time, especially in the 8-12GHz frequency band, the reflection loss of the material is relatively high, which affects its application value.
CoFe2O4 nanosheets were prepared by hydrothermal method, and TiO2 nanoparticles were loaded on their surface to control the load and crystal form of TiO2 nanoparticles, avoid the formation of anatase-type TiO2, and combine with polyaniline coating to prepare excellent electromagnetic shielding with Effective composite wave absorbing material.
It has achieved electromagnetic shielding performance of 60-70dB and low reflection loss of -15-50dB in the 8-12GHz frequency band, which significantly improves the electromagnetic shielding performance of the material and is suitable for electronic equipment.
Smart Images

Figure BDA0004389380700000071 
Figure BDA0004389380700000072 
Figure BDA0004389380700000081
Abstract
Description
Background Art
[0001] The chemical formula of spinel ferrite is ABO4, where A is Mn 2+ 、Ni 2+ 、Co 2+ , Fe 2+ 、Zn 2+ Equivalent metal ions; B is Fe 3+ 、A1 3+ Cr 3+ It is a typical soft ferrite and a ferromagnetic material. It has trivalent metal ions and the same crystal structure as spinel MgAO4. It has excellent magnetic properties and chemical stability, high resistivity and excellent wave absorbing properties, making it a hot research material for electromagnetic shielding materials and stealth material absorbers.
[0002] Chinese patent CN 115140781 A discloses a new type of absorbing material and preparation method, which improves electromagnetic wave absorption performance by compounding materials and controlling the morphology of materials. Nano-sheet MnFe2O4 is prepared by hydrothermal method, which overlaps to form a three-dimensional network structure, and nano-NiMoO4 is loaded on the nano-sheet by microwave hydrothermal method, and interface polarization is generated between the two to improve the absorbing performance. The three-dimensional material structure is conducive to reducing the surface reflection of electromagnetic waves and reducing the dielectric constant and refractive index of the material.
[0003] Chinese patent CN 103012786 A discloses a method for preparing a graphene / CoFe2O4 / polyaniline composite absorbing material. The present invention first prepares graphene using carbon nanotubes with a diameter of 0 to 50 nm as raw materials, then uses Co(NO3)2·6H2O and Fe(NO3)3·9H2O as raw materials to prepare CoFe2O4 by a sol-gel self-propagating combustion method, and finally uses the prepared graphene, CoFe2O4 and aniline monomer as raw materials to prepare a graphene / CoFe2O4 / polyaniline composite material by an in-situ polymerization method. The composite material has good electrical conductivity, magnetic properties and stability, and has important application value in the fields of microwave absorption and electromagnetic shielding.
[0004] Foreign patent IN201811023894A discloses an improved composition for EMI shielding, consisting of: polymer-modified nanoferrite, the content of which is 20 to 90wt%. Conductive polymer is in the range of 10 to 80 weight%. The total shielding efficiency of the composition is in the range of 7 to 44dB. And the surface of the nanoferrite particles is modified with an insulating polymer polymethyl methacrylate (PMMA) to enhance dispersibility and morphology control; a composite comprising PMMA-modified nanoferrite and polyaniline is provided for effectively absorbing electromagnetic waves at X-band frequencies (8 to 12GHz).
[0005] How to seek the combination of materials and preparation methods to obtain better electromagnetic shielding materials remains the focus of research. Summary of the invention
[0006] Based on the needs and trends of the prior art, the present invention proposes a composite absorbing material, an electromagnetic shielding film and a preparation method thereof with high shielding efficiency and low reflection loss, and prepares an electromagnetic shielding film with excellent electromagnetic shielding effect and low reflection loss in the 8-12 GHz frequency band, which can be widely used in electronic equipment.
[0007] In order to solve the technical problem of this application, the present invention provides the following technical solutions:
[0008] A method for preparing a composite absorbing material with high electromagnetic shielding effectiveness and low reflection loss comprises the following steps:
[0009] (1) dissolving 0.1 mol of cobalt nitrate and 0.2 mol of ferric nitrate in 120-150 mL of deionized water, stirring and dissolving to obtain a mixed solution; dissolving 0.05 mol of 1,2-cyclohexanediaminetetraacetic acid disodium in 30-50 mL of deionized water to obtain a 1,2-cyclohexanediaminetetraacetic acid disodium solution; then slowly adding the 1,2-cyclohexanediaminetetraacetic acid disodium solution to the mixed solution, and transferring the mixture to a hydrothermal reactor, performing a hydrothermal reaction at 190-210° C. for 12-15 hours, and after the reaction is completed, filtering, washing, and drying the hydrothermal reaction solution to obtain CoFe2O4 nanosheets;
[0010] (2) placing the CoFe2O4 nanosheets prepared in step (1) in a quartz tube furnace, heating the furnace to 450-500° C., and heat treating the nanosheets in an air atmosphere for 2-3 h;
[0011] (3) Dispersing the CoFe2O4 nanosheets in 100 mL of deionized water, then adding 5 to 10 mL of anhydrous titanium chloride and stirring evenly, then transferring the mixture to a hydrothermal reactor for a hydrothermal reaction at 115 to 125° C. for 4 to 6 hours. After the reaction is completed, filtering, washing, and drying the hydrothermal reaction solution to obtain TiO2 nanoparticles@CoFe2O4 nanosheets;
[0012] (4) Weigh 10 g of TiO2 nanoparticles @ CoFe2O4 nanosheets and place them in 100 mL of dilute hydrochloric acid solution and ultrasonically disperse them for 10 to 20 minutes; add 10 to 13 mL of aniline monomer; place the reaction container in an ice water bath and stir, continue to add 10 to 15 g of ammonium persulfate solution and 0.5 to 1 mL of dodecylbenzene sulfonic acid, react for 5 to 9 hours, filter, wash and dry the reaction solution to obtain a composite absorber material of polyaniline-coated TiO2 nanoparticles @ CoFe2O4 nanosheets.
[0013] In the present application, anhydrous titanium chloride is used as a raw material for hydrothermal synthesis of TiO2 nanoparticles, and by controlling the hydrothermal temperature at 115-125°C, anatase TiO2 can be prepared; and by controlling the amount of anhydrous titanium chloride, the TiO2 nanoparticles are loaded on CoFe2O4 nanosheets, and the loading amount of the TiO2 nanoparticles is controlled to avoid the formation of TiO2 nanoparticles fully covering the CoFe2O4 nanosheets, that is, to avoid the formation of a core-shell structure.
[0014] A composite wave absorbing material with high electromagnetic shielding effectiveness and low reflection loss is prepared by the above method.
[0015] Furthermore, the particle size of the composite absorbing material is 0.5-1.2 μm.
[0016] The applicant found in the process of research that the loading amount of TiO2 nanoparticles has a significant effect on the shielding efficiency of the absorbing material; the electromagnetic shielding efficiency of the CoFe2O4 nanosheets fully covered by TiO2 nanoparticles is significantly reduced. In addition, the TiO2 crystal form usually obtained by hydrothermal reaction synthesis of TiO2 is anatase phase, rutile phase and mixed phase; however, the higher the content of rutile phase, the higher the reflection loss of the absorbing material, so the applicant controls the hydrothermal temperature at 115-125°C, which can effectively avoid the formation of anatase TiO2.
[0017] Furthermore, the structure of the composite absorbing material is that TiO2 nanoparticles are loaded on CoFe2O4 nanosheets with a loading amount of 30-40%.
[0018] Furthermore, the content of rutile TiO2 in the composite absorbing material is greater than 95%.
[0019] In the prior art, a CoFe2O4 and TiO2 composite material is usually prepared first and then subjected to a heat treatment step at 450-500°C. However, when subjected to heat treatment at 450-500°C, the crystal phase of TiO2 will be transformed into anatase TiO2. In the present application, a separate heat treatment step is performed immediately after the CoFe2O4 nanosheets are prepared, so that the crystal phase of TiO2 is prevented from being transformed into anatase TiO2, which causes an increase in the reflection loss of the absorbing material.
[0020] Furthermore, in step (1), the time for slowly adding the 1,2-cyclohexanediaminetetraacetic acid disodium solution to the mixed solution is controlled to be 30 to 60 seconds.
[0021] In step (1), the use of disodium 1,2-cyclohexanediaminetetraacetate can effectively control the grain size and morphology of CoFe2O4, thereby obtaining CoFe2O4 with a nano-sheet morphology, thereby increasing the surface area of CoFe2O4 and providing a guarantee for the subsequent loading of nano-TiO2 on its surface.
[0022] An electromagnetic shielding film using the above-mentioned composite absorbing material as a component, in parts by weight, the electromagnetic shielding film comprises 80-90 parts of polyvinylidene chloride resin, 10-20 parts of composite absorbing material, and 30-50 parts of boron nitride powder; the preparation steps of the electromagnetic shielding film are as follows: (1) heating 200-250 parts of N,N-dimethylformamide to 50-70°C, adding polyvinylidene chloride resin particles, stirring to dissolve; then adding composite absorbing material and boron nitride powder, continuing to stir to obtain a mixed solution; (2) spin coating the mixed solution on the surface of a substrate, placing the substrate in an oven at 100-120°C and heating for 2-3 hours, and cooling to room temperature with the oven.
[0023] Furthermore, the particle size of the boron nitride powder is 50 to 100 μm. Boron nitride is a material with excellent thermal conductivity and mechanical properties. As a filler in the electromagnetic shielding film, it can significantly improve its thermal conductivity and the hardness and wear resistance of the electromagnetic shielding film; and effectively improve the service life of the electromagnetic shielding film.
[0024] Furthermore, the thickness of the electromagnetic shielding film can be obtained by multiple spin coatings; or can be obtained by placing the mixed solution in a mold of a suitable size.
[0025] Furthermore, the preparation steps of the electromagnetic shielding film are as follows: (1) heating 200 to 250 parts of N,N-dimethylformamide to 50 to 70°C, adding polyvinylidene chloride resin particles, and stirring to dissolve; then adding composite absorbing material and boron nitride powder, and continuing to stir to obtain a mixed solution; (2) pouring the above mixed solution into a mold, placing the substrate in an oven at 100 to 120°C and heating for 2 to 3 hours, and cooling to room temperature with the oven; separating the electromagnetic shielding film from the mold.
[0026] Furthermore, the electromagnetic shielding film also includes 1 to 5 parts of antioxidants and / or anti-ultraviolet agents, wherein the antioxidant is selected from one or more of dilauryl thiodipropionate and propylene pentaerythritol ester; and the anti-ultraviolet agent is selected from one or more of UV531 and UV-9.
[0027] Furthermore, the electromagnetic shielding effectiveness of the electromagnetic shielding film is 60 to 70 dB, and the reflection loss ranges from -15 to -50 dB at 2 to 18 GHz.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) The specific structure of the composite absorbing material prepared by the present invention is a shell structure of polyaniline-coated TiO2 nanoparticles@CoFe2O4 nanosheets, in which TiO2 nanoparticles are loaded on CoFe2O4 nanosheets; and by controlling the loading amount of TiO2 nanoparticles and the formation of anatase TiO2 as much as possible in the process, its electromagnetic shielding performance can be effectively improved.
[0030] (2) The composite absorbing material of the present application has excellent electromagnetic shielding effect and low reflection loss in the 8-12 GHz frequency band. Its electromagnetic shielding efficiency is 60-70 dB, and its reflection loss range is -15--50 dB in the 2-18 GHz frequency band. It can be widely used in electronic equipment products. DETAILED DESCRIPTION
[0031] The technical solution of the present invention is further described below in conjunction with specific examples. Those skilled in the art should understand that the specific implementation methods are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0032] Example 1
[0033] A method for preparing a wave absorbing material with high electromagnetic shielding effectiveness and low reflection loss comprises the following steps:
[0034] (1) dissolving 0.1 mol of cobalt nitrate and 0.2 mol of ferric nitrate in 120 mL of deionized water, stirring and dissolving to obtain a mixed solution; dissolving 0.05 mol of 1,2-cyclohexanediaminetetraacetic acid disodium in 30 mL of deionized water to obtain a 1,2-cyclohexanediaminetetraacetic acid disodium solution; then slowly adding the 1,2-cyclohexanediaminetetraacetic acid disodium solution to the mixed solution, and transferring the mixture to a hydrothermal reactor, performing a hydrothermal reaction at 190° C. for 12 hours, and after the reaction is completed, filtering, washing, and drying the hydrothermal reaction solution to obtain CoFe2O4 nanosheets;
[0035] (2) placing the CoFe2O4 nanosheets prepared in step (1) in a quartz tube furnace, heating to 450°C, and heat treating in an air atmosphere for 2 hours;
[0036] (3) Dispersing the CoFe2O4 nanosheets in 100 mL of deionized water, then adding 5 mL of anhydrous titanium chloride and stirring evenly, then transferring the mixture into a hydrothermal reactor for a hydrothermal reaction at 115° C. for 4 h. After the reaction is completed, filtering, washing, and drying the hydrothermal reaction solution to obtain TiO2 nanoparticles@CoFe2O4 nanosheets;
[0037] (4) Weigh 10 g of TiO2 nanoparticles @ CoFe2O4 nanosheets and place them in 100 mL of dilute hydrochloric acid solution and ultrasonically disperse them for 10 minutes; add 10 mL of aniline monomer; place the reaction container in an ice water bath and stir, continue to add 10 g of ammonium persulfate solution and 0.5 mL of dodecylbenzene sulfonic acid, react for 5 hours, filter, wash and dry the reaction solution to obtain a composite absorber material of polyaniline-coated TiO2 nanoparticles @ CoFe2O4 nanosheets.
[0038] Example 2
[0039] A method for preparing a wave absorbing material with high electromagnetic shielding effectiveness and low reflection loss comprises the following steps:
[0040] (1) dissolving 0.1 mol of cobalt nitrate and 0.2 mol of ferric nitrate in 150 mL of deionized water, stirring and dissolving to obtain a mixed solution; dissolving 0.05 mol of 1,2-cyclohexanediaminetetraacetic acid disodium in 50 mL of deionized water to obtain a 1,2-cyclohexanediaminetetraacetic acid disodium solution; then slowly adding the 1,2-cyclohexanediaminetetraacetic acid disodium solution to the mixed solution, and transferring the mixture to a hydrothermal reactor, performing a hydrothermal reaction at 210° C. for 15 hours, and after the reaction is completed, filtering, washing, and drying the hydrothermal reaction solution to obtain CoFe2O4 nanosheets;
[0041] (2) placing the CoFe2O4 nanosheets prepared in step (1) in a quartz tube furnace, heating to 500°C, and heat treating in an air atmosphere for 3 hours;
[0042] (3) Dispersing the CoFe2O4 nanosheets in 100 mL of deionized water, then adding 10 mL of anhydrous titanium chloride and stirring evenly, then transferring the mixture into a hydrothermal reactor for a hydrothermal reaction at 125° C. for 6 h. After the reaction is completed, filtering, washing, and drying the hydrothermal reaction solution to obtain TiO2 nanoparticles@CoFe2O4 nanosheets;
[0043] (4) Weigh 10 g of TiO2 nanoparticles @ CoFe2O4 nanosheets into 100 mL of dilute hydrochloric acid solution and disperse it ultrasonically for 20 min; add 13 mL of aniline monomer; place the reaction container in an ice water bath and stir, continue to add 10-15 g of ammonium persulfate solution and 1 mL of dodecylbenzene sulfonic acid, react for 9 h, filter, wash and dry the reaction solution to obtain a composite absorber of polyaniline-coated TiO2 nanoparticles @ CoFe2O4 nanosheets.
[0044] Example 3
[0045] A method for preparing a wave absorbing material with high electromagnetic shielding effectiveness and low reflection loss comprises the following steps:
[0046] (1) dissolving 0.1 mol of cobalt nitrate and 0.2 mol of ferric nitrate in 130 mL of deionized water, stirring and dissolving to obtain a mixed solution; dissolving 0.05 mol of 1,2-cyclohexanediaminetetraacetic acid disodium in 40 mL of deionized water to obtain a 1,2-cyclohexanediaminetetraacetic acid disodium solution; then slowly adding the 1,2-cyclohexanediaminetetraacetic acid disodium solution to the mixed solution, and transferring the mixture to a hydrothermal reactor, performing a hydrothermal reaction at 200° C. for 13 hours, and after the reaction is completed, filtering, washing, and drying the hydrothermal reaction solution to obtain CoFe2O4 nanosheets;
[0047] (2) placing the CoFe2O4 nanosheets prepared in step (1) in a quartz tube furnace, heating to 480° C., and heat treating in an air atmosphere for 2.5 h;
[0048] (3) Dispersing the CoFe2O4 nanosheets in 100 mL of deionized water, then adding 7 mL of anhydrous titanium chloride and stirring evenly, then transferring the mixture into a hydrothermal reactor for a hydrothermal reaction at 120° C. for 5 h. After the reaction is completed, filtering, washing, and drying the hydrothermal reaction solution to obtain TiO2 nanoparticles@CoFe2O4 nanosheets;
[0049] (4) Weigh 10 g of TiO2 nanoparticles @ CoFe2O4 nanosheets into 100 mL of dilute hydrochloric acid solution and disperse it ultrasonically for 15 min; add 13 mL of aniline monomer; place the reaction container in an ice water bath and stir, continue to add 12 g of ammonium persulfate solution and 0.7 mL of dodecylbenzene sulfonic acid, react for 7 h, filter, wash and dry the reaction solution to obtain a composite absorber of polyaniline-coated TiO2 nanoparticles @ CoFe2O4 nanosheets.
[0050] For better explanation, the applicant uses Example 3 as a benchmark, changes the process parameters in the preparation process, and further investigates the influence of the process parameters on the performance of the composite absorbing material.
[0051] Comparative Example 1
[0052] A method for preparing a composite absorbing material with high shielding efficiency and low reflection loss comprises the following steps:
[0053] (1) dissolving 0.1 mol of cobalt nitrate and 0.2 mol of ferric nitrate in 130 mL of deionized water, stirring and dissolving to obtain a mixed solution; dissolving 0.05 mol of 1,2-cyclohexanediaminetetraacetic acid disodium in 40 mL of deionized water to obtain a 1,2-cyclohexanediaminetetraacetic acid disodium solution; then slowly adding the 1,2-cyclohexanediaminetetraacetic acid disodium solution to the mixed solution, and transferring the mixture to a hydrothermal reactor, performing a hydrothermal reaction at 200° C. for 13 hours, and after the reaction is completed, filtering, washing, and drying the hydrothermal reaction solution to obtain CoFe2O4 nanosheets;
[0054] (2) placing the CoFe2O4 nanosheets prepared in step (1) in a quartz tube furnace, heating to 480° C., and heat treating in an air atmosphere for 2.5 h;
[0055] (3) Dispersing the CoFe2O4 nanosheets in 100 mL of deionized water, then adding 20 mL of anhydrous titanium chloride and stirring evenly, then transferring the mixture into a hydrothermal reactor for hydrothermal reaction at 120° C. for 5 h. After the reaction is completed, filtering, washing, and drying the hydrothermal reaction solution to obtain TiO2 nanoparticles@CoFe2O4 nanosheets;
[0056] (4) Weigh 10 g of TiO2 nanoparticles @ CoFe2O4 nanosheets into 100 mL of dilute hydrochloric acid solution and disperse it ultrasonically for 15 min; add 13 mL of aniline monomer; place the reaction container in an ice water bath and stir, continue to add 12 g of ammonium persulfate solution and 0.7 mL of dodecylbenzene sulfonic acid, react for 7 h, filter, wash and dry the reaction solution to obtain a composite absorber of polyaniline-coated TiO2 nanoparticles @ CoFe2O4 nanosheets.
[0057] Comparative Example 2
[0058] A method for preparing a composite absorbing material with high shielding efficiency and low reflection loss comprises the following steps:
[0059] (1) dissolving 0.1 mol of cobalt nitrate and 0.2 mol of ferric nitrate in 130 mL of deionized water, stirring and dissolving to obtain a mixed solution; dissolving 0.05 mol of 1,2-cyclohexanediaminetetraacetic acid disodium in 40 mL of deionized water to obtain a 1,2-cyclohexanediaminetetraacetic acid disodium solution; then slowly adding the 1,2-cyclohexanediaminetetraacetic acid disodium solution to the mixed solution, and transferring the mixture to a hydrothermal reactor, performing a hydrothermal reaction at 200° C. for 13 hours, and after the reaction is completed, filtering, washing, and drying the hydrothermal reaction solution to obtain CoFe2O4 nanosheets;
[0060] (2) placing the CoFe2O4 nanosheets prepared in step (1) in a quartz tube furnace, heating to 480° C., and heat treating in an air atmosphere for 2.5 h;
[0061] (3) Dispersing CoFe2O4 nanosheets in 100 mL of deionized water, then adding 7 mL of anhydrous titanium chloride and stirring evenly, then transferring to a hydrothermal reactor for hydrothermal reaction at 180° C. for 5 h. After the reaction is completed, filtering, washing, and drying the hydrothermal reaction liquid to obtain TiO2 nanoparticles@CoFe2O4 nanosheets;
[0062] (4) Weigh 10 g of TiO2 nanoparticles @ CoFe2O4 nanosheets into 100 mL of dilute hydrochloric acid solution and disperse it ultrasonically for 15 min; add 13 mL of aniline monomer; place the reaction container in an ice water bath and stir, continue to add 12 g of ammonium persulfate solution and 0.7 mL of dodecylbenzene sulfonic acid, react for 7 h, filter, wash and dry the reaction solution to obtain a composite absorber of polyaniline-coated TiO2 nanoparticles @ CoFe2O4 nanosheets.
[0063] 1. The products of the preparation processes of Examples 1-3 and Comparative Examples 1-2 were tested and characterized. The specific data are recorded in Table 1.
[0064] Table 1
[0065]
[0066] From the experimental data in Table 1, it can be seen that the difference between Comparative Example 1 and Example 3 lies in the amount of anhydrous titanium chloride used. The more anhydrous titanium chloride is used, the more TiO2 nanoparticles are generated and loaded on the surface of the CoFe2O4 nanosheets during the hydrothermal reaction, which leads to an increase in the loading rate of TiO2 nanoparticles. The difference between Comparative Example 2 and Example 3 lies in the higher temperature of the hydrothermal reaction, which leads to an increase in the content of anatase TiO2 and a decrease in the content of rutile TiO2.
[0067] 2. In order to test the electromagnetic shielding effectiveness and reflection loss of the composite absorbing material prepared by the technical party of the present invention, the composite absorbing material prepared according to the embodiment and the comparative example is used as a component of the electromagnetic shielding film. In parts by weight, the electromagnetic shielding film includes 85 parts of polyvinylidene chloride resin, 14 parts of composite absorbing material, and 38 parts of boron nitride powder; the preparation steps of the electromagnetic shielding film are as follows: (1) Heat 220 parts of N,N-dimethylformamide to 60°C, add polyvinylidene chloride resin particles, and stir to dissolve; then add the composite absorbing material and boron nitride powder, continue to stir to obtain a mixed solution; (2) Pour the above mixed solution into a mold (the mold size is 300mm×200mm×6mm), put the substrate into an oven at 110°C and heat for 2h, and cool to room temperature with the furnace; separate the electromagnetic shielding film from the mold.
[0068] The electromagnetic shielding effectiveness of the material was tested in its original state and after external force (bending 50 times) in accordance with the standard "SJ20524-95 Measurement method for shielding effectiveness of materials". The test data are recorded in Table 2, and the measured reflection loss data are recorded in Tables 3-4.
[0069] Table 2
[0070]
[0071] According to the data in Table 2, the electromagnetic shielding effectiveness of the electromagnetic shielding film prepared in this embodiment is 60-70 dB, showing excellent electromagnetic shielding performance. Moreover, the material still maintains excellent shielding performance after being bent 50 times, and the electromagnetic shielding effectiveness decreases by only about 1 dB compared with the original material state.
[0072] The decrease in the data of comparative example 1 indicates that the higher the loading rate of TiO2 nanoparticles, the lower the electromagnetic shielding efficiency of the composite absorbing material; the decrease in the data of comparative example 2 indicates that the lower the content of rutile TiO2, the more unfavorable it is for the electromagnetic shielding efficiency of the composite absorbing material.
[0073] Table 3
[0074]
[0075] Table 4
[0076]
[0077] According to the data in Table 3-4, the reflection loss range of the shell material prepared in this embodiment at 2 to 18 GHz is -15 to -50 dB. It reaches about -50 dB near 13 GHz, indicating that the composite absorbing material prepared by the technical solution of this application has excellent performance in the 2 to 18 GHz frequency band. In contrast, the reflection loss range of the comparative example at 2 to 18 GHz is -10 to -35 dB, and the overall performance is far lower than the level of this application.
[0078] In summary, the embodiments of the present invention prepare a composite absorbing material with high electromagnetic shielding effectiveness and low reflection loss, which can be widely used in electronic products and equipment.
[0079] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a composite absorbing material with high electromagnetic shielding effectiveness and low reflection loss, characterized in that: The steps include: (1) dissolving 0.1 mol of cobalt nitrate and 0.2 mol of ferric nitrate in 120-150 mL of deionized water, stirring and dissolving to obtain a mixed solution; dissolving 0.05 mol of 1,2-cyclohexanediaminetetraacetic acid disodium in 30-50 mL of deionized water to obtain a 1,2-cyclohexanediaminetetraacetic acid disodium solution; then slowly adding the 1,2-cyclohexanediaminetetraacetic acid disodium solution to the mixed solution, and transferring the mixture to a hydrothermal reactor, performing a hydrothermal reaction at 190-210° C. for 12-15 hours, and after the reaction is completed, filtering, washing, and drying the hydrothermal reaction solution to obtain CoFe2O4 nanosheets; (2) placing the CoFe2O4 nanosheets prepared in step (1) in a quartz tube furnace, heating the furnace to 450-500° C., and heat treating the nanosheets in an air atmosphere for 2-3 h; (3) Dispersing the CoFe2O4 nanosheets in 100 mL of deionized water, then adding 5 to 10 mL of anhydrous titanium chloride and stirring evenly, then transferring the mixture to a hydrothermal reactor for a hydrothermal reaction at 115 to 125° C. for 4 to 6 hours. After the reaction is completed, filtering, washing, and drying the hydrothermal reaction solution to obtain TiO2 nanoparticles@CoFe2O4 nanosheets; (4) Weigh 10 g of TiO2 nanoparticles @ CoFe2O4 nanosheets and place them in 100 mL of dilute hydrochloric acid solution and ultrasonically disperse them for 10 to 20 minutes; add 10 to 13 mL of aniline monomer; place the reaction container in an ice water bath and stir, continue to add 10 to 15 g of ammonium persulfate solution and 0.5 to 1 mL of dodecylbenzene sulfonic acid, react for 5 to 9 hours, filter, wash and dry the reaction solution to obtain a composite absorber material of polyaniline-coated TiO2 nanoparticles @ CoFe2O4 nanosheets.
2. The method for preparing a composite absorbing material with high electromagnetic shielding effectiveness and low reflection loss according to claim 1, characterized in that: In step (1), the time for slowly adding the 1,2-cyclohexanediaminetetraacetic acid disodium solution into the mixed solution is controlled to be 30 to 60 seconds.
3. A composite absorbing material with high electromagnetic shielding effectiveness and low reflection loss, characterized in that: The composite absorbing material is prepared by the preparation method according to any one of claims 1 to 2.
4. The composite absorbing material with high electromagnetic shielding effectiveness and low reflection loss according to claim 3, characterized in that: The particle size of the composite wave absorbing material is 0.5-1.2 μm.
5. The composite absorbing material with high electromagnetic shielding effectiveness and low reflection loss according to claim 3, characterized in that: The structure of the composite wave absorbing material is that TiO2 nanoparticles are loaded on CoFe2O4 nanosheets in a loading amount of 30-40%; the content of rutile TiO2 in the composite wave absorbing material is greater than 95%.
6. An electromagnetic shielding film comprising the composite absorbing material prepared according to any one of claims 1 to 2 or the composite absorbing material according to any one of claims 3 to 5, characterized in that: In parts by weight, the electromagnetic shielding film comprises 80-90 parts of polyvinylidene chloride resin, 10-20 parts of composite absorbing material, and 30-50 parts of boron nitride powder. The preparation steps of the electromagnetic shielding film are as follows: (1) heating 200-250 parts of N,N-dimethylformamide to 50-70°C, adding polyvinylidene chloride resin particles, and stirring to dissolve; then adding composite absorbing material and boron nitride powder, and continuing to stir to obtain a mixed solution; (2) spin coating the mixed solution on the surface of a substrate, placing the substrate in an oven at 100-120°C and heating it for 2-3 hours, and cooling it to room temperature with the oven.
7. The electromagnetic shielding film according to claim 6, characterized in that: The particle size of the boron nitride powder is 50-100 μm; the thickness of the electromagnetic shielding film can be obtained by multiple spin coatings; or by placing the mixed solution in a mold of a suitable size.
8. The electromagnetic shielding film according to claim 6, characterized in that: The preparation steps of the electromagnetic shielding film are as follows: (1) heating 200 to 250 parts of N,N-dimethylformamide to 50 to 70°C, adding polyvinylidene chloride resin particles, and stirring to dissolve; then adding composite absorbing material and boron nitride powder, and continuing to stir to obtain a mixed solution; (2) pouring the above mixed solution into a mold, placing the substrate in an oven at 100 to 120°C and heating for 2 to 3 hours, and cooling to room temperature with the oven; separating the electromagnetic shielding film from the mold.
9. The electromagnetic shielding film according to claim 6 or 8, characterized in that: The electromagnetic shielding film also includes 1 to 5 parts of antioxidant and / or anti-ultraviolet agent, wherein the antioxidant is selected from one or more of dilauryl thiodipropionate and propylene pentaerythritol ester; and the anti-ultraviolet agent is selected from one or more of UV531 and UV-9.
10. The electromagnetic shielding film according to claim 6 or 8, characterized in that: The electromagnetic shielding effectiveness of the electromagnetic shielding film is 60-70 dB, and the reflection loss ranges from -15 to -50 dB at 2-18 GHz.
Citation Information
Patent Citations
Preparation method of graphene / CoFe2O4 / polyaniline composite absorbing material
CN103012786A
Efficient microwave absorbing material
CN115140781A
An improved composition for electromagnetic interference (EMI) schielding and a process for the preparation thereof
IN201811023894A
MIXED CRYSTAL TiO2 / BiOBr COMPOSITE AND PREPARATION METHOD AND APPLICATION THEREOF
AU2020102258A4
Wave-absorbing composite material
CN104608430A