Aggregation-induced emission carbon dots, preparation method and application thereof
By sonicating TPE, Er(NO3)3 and Yb(NO3)3 in glacial acetic acid, hydrothermal reaction and drying, rare earth-doped aggregation-induced luminescent carbon dots were prepared, and the carbon dot material was solved in the aggregation state. The problem of fluorescence quenching achieves efficient cell imaging and biosafety, overcomes the ACQ effect, and demonstrates strong fluorescence signals and long lifespan.
Patent Information
- Application Number
- CN202311115221.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-08-31
AI Technical Summary
The existing carbon dot materials have aggregation fluorescence quenching (ACQ) effect in the aggregated state, which limits their application in biological imaging. There are few researches on rare earth-doped AIE carbon dots and lacks effective solutions.
TPE, Er(NO3)3 and Yb(NO3)3 were used to sonicate in glacial acetic acid, and hydrothermal reaction was carried out, followed by cooling and deionized water to form a suspension. After sonication and centrifugation, doped Aggregation of rare earth elements induced luminescent carbon dots.
The prepared carbon dots have high emission signal intensity, long fluorescence lifetime and high quantum efficiency. They overcome the ACQ effect, are suitable for cell imaging, and show biosafety and selective imaging characteristics in zebrafish and zebrafish eggs.
Smart Images

Figure CN117143597B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of nanomaterials, and in particular to aggregation-induced luminescence carbon dots, a preparation method and application thereof. Background Art
[0002] Photoluminescent materials have been gaining more and more attention in recent years because of their wide applications in chemical probes, sensors, information storage, and bio-imaging. However, this type of material widely suffers from the aggregation fluorescence quenching (ACQ) effect, that is, when in an aggregated state or solid state, its fluorescence will be significantly weakened or even disappear. This phenomenon has greatly limited the development and application of photoluminescent materials. In contrast to the ACQ material phenomenon, Tang Benzhong et al. confirmed the existence of the aggregation-induced emission (AIE) effect in 2001, in which bright fluorescence can be observed in the aggregated state. This discovery breaks the shackles of traditional concepts and opens up new avenues for the design and functional development of luminescent materials.
[0003] The molecular structure of luminescent materials with AIE effect contains several freely rotating aromatic groups at low concentrations. Therefore, at high concentrations or in solid state, non-radiative decay is blocked due to the restriction of intramolecular rotation (RIR) caused by the π-π stacking effect between molecules. Therefore, when AIE luminescent materials are more aggregated, they show stronger fluorescence intensity, overcoming all ACQ effects.
[0004] The successful realization of biological imaging requires fluorescent probes with good photostability, high definition, good dispersibility in water and biocompatibility. As an important member of the carbon material family, carbon dots (CDs) have attracted much attention due to their unique optical properties and simple synthesis methods. Carbon dots do not have the toxicity problem caused by the leakage of heavy metal ions of inorganic quantum dots and have good biocompatibility. However, the above-mentioned ACQ problem still exists, which will cause the loss of sufficient sensitivity to monitor small changes in biological imaging. However, AIE carbon dots not only have the common advantages of ordinary carbon dots, but also emit bright fluorescence even in the aggregated state. Therefore, AIE carbon dots are a good substitute for fluorescent labels for biological imaging.
[0005] Among many luminescent materials, rare earth (RE) complexes usually have high emission efficiency in aggregated and solid states, and this luminescent property is very similar to AIE luminophores. The difference is that rare earth luminescence is a sensitization process in which energy is transferred from the excited triplet state of the ligand to the excited state of the rare earth ion (T1-RE*). On the other hand, rare earth ions have unique luminescence properties, high-intensity emission signals, long fluorescence lifetimes, and high quantum efficiency. However, there are few reports on rare earth-doped AIE carbon dots. The combination of rare earth elements and AIE carbon dots is expected to bring new prospects for bioimaging applications. But there is no publicly available reliable solution. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide an aggregation-induced luminescence carbon dot, a preparation method and application thereof in view of the deficiencies in the above-mentioned prior art.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing aggregation-induced emission carbon dots, comprising the following steps:
[0008] 1) Combine TPE, Er(NO 3 ) 3 and Yb(NO 3 ) 3 Dissolve in glacial acetic acid and sonicate to obtain a mixture;
[0009] 2) transferring the mixture obtained in step 1) into a reaction kettle and performing a hydrothermal reaction under heating;
[0010] 3) After the reaction is completed, the mixture is cooled to room temperature, and deionized water is added to the obtained product to form a suspension;
[0011] 4) After ultrasonic treatment of the suspension, centrifugation is performed to collect the solid product; the ultrasonic treatment and centrifugation steps are repeated, and the obtained solid product is vacuum dried to obtain aggregation-induced emission carbon dots.
[0012] Preferably, step 1) is specifically: 166-664 mg TPE, 11.6-42.6 mg Er(NO 3 ) 3 and 65-260mgYb(NO 3 ) 3 Dissolve in 20-40 mL of glacial acetic acid and sonicate for 15-60 minutes to obtain a mixture.
[0013] Preferably, step 1) is specifically as follows: 332 mg TPE, 21.3 mg Er(NO 3 ) 3 and 129.2 mg Yb(NO 3 ) 3 The solution was dissolved in 40 mL of glacial acetic acid and sonicated for 30 minutes to obtain a mixture.
[0014] Preferably, step 2) is specifically: transferring the mixture obtained in step 1) into a reaction kettle and reacting at 170-200° C. for 8-24 hours.
[0015] Preferably, step 2) is specifically as follows: transferring the mixture obtained in step 1) into an 80 mL polytetrafluoroethylene-lined autoclave, and reacting at 180° C. for 16 hours.
[0016] Preferably, step 3) specifically comprises: cooling to room temperature after the reaction is completed, and adding 200 mL of deionized water to the obtained product to form a suspension.
[0017] Preferably, step 4) is specifically as follows: ultrasonically treat the suspension for 2-10 minutes, centrifuge at 5000-20000 rpm for 5-20 minutes, and collect the solid product; repeat the ultrasonic treatment and centrifugation steps 2-5 times, and vacuum dry the solid product at 50-70°C to obtain aggregation-induced emission carbon dots.
[0018] Preferably, step 4) is specifically as follows: ultrasonically treat the suspension for 5 minutes, centrifuge at 10,000 rpm for 10 minutes, and collect the solid product; repeat the ultrasonic treatment and centrifugation steps three times, and vacuum dry the solid product at 60° C. to obtain aggregation-induced emission carbon dots.
[0019] The present invention also provides an aggregation-induced emission carbon dot, which is prepared by the method as described above.
[0020] The present invention also provides an application of the aggregation-induced emission carbon dots prepared by the method described above in cell imaging.
[0021] The beneficial effects of the present invention are:
[0022] The present invention proposes a method for synthesizing AIE carbon dots doped with rare earth elements Yb and Er. The carbon dots have aggregation-induced emission characteristics, can overcome the problem of aggregation fluorescence quenching (ACQ) effect of traditional carbon dot materials, have high emission signal intensity, long fluorescence lifetime, and high quantum efficiency, can be well applied to cell imaging, and have proved their biosafety in long-term imaging of zebrafish and zebrafish eggs, and have the characteristics of selective imaging of the lens and digestive system of zebrafish. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The dispersion effect of the carbon dots prepared in Example 1 in the solvent;
[0024] Figure 2 This is a transmission electron microscope photo of the carbon dots prepared in Example 1;
[0025] Figure 3 X-ray diffraction spectrum (a), Raman spectrum (b) and Fourier transform infrared spectrum (c) of the carbon dots prepared in Example 1;
[0026] Figure 4 X-ray photoelectron diffraction spectrum (XPS) of the carbon dots prepared in Example 1;
[0027] Figure 5 The fluorescence spectra of the carbon dots prepared in Example 1 at different excitation wavelengths;
[0028] Figure 6 This is an image of the carbon dots prepared in Example 1 on the cell nucleus;
[0029] Figure 7 The imaging results of the carbon dots prepared in Example 1 on zebrafish embryos (Embruso) and larvae (Larval zebranfish). DETAILED DESCRIPTION
[0030] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.
[0031] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0032] The test methods used in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are all commercially available unless otherwise specified. In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0033] Example 1
[0034] An aggregation-induced emission carbon dot, the preparation method of which comprises the following steps:
[0035] 1) 332 mg TPE, 21.3 mg Er(NO 3 ) 3 and 129.2 mg Yb(NO 3 ) 3 The mixture was dissolved in 40 mL of glacial acetic acid and sonicated for 30 min to obtain a mixture;
[0036] 2) transferring the mixture obtained in step 1) into an 80 mL polytetrafluoroethylene-lined autoclave and reacting at 180° C. for 16 hours;
[0037] 3) After the reaction is completed, the mixture is cooled to room temperature, and 200 mL of deionized water is added to the obtained product to form a suspension;
[0038] 4) After ultrasonic treatment of the suspension for 5 minutes, centrifugation was performed at 10,000 rpm for 10 minutes to collect the solid product; the ultrasonic treatment and centrifugation steps were repeated three times, and the solid product was vacuum dried at 60° C. to obtain yellow aggregation-induced emission carbon dots AIE-CDs (hereinafter referred to as carbon dots).
[0039] Since the carbon dot powder has poor dispersibility in water, it is difficult to conduct experiments. In order to solve this problem, the carbon dot powder was dissolved in DMSO to a concentration of 1 mg / mL, and deionized water was added again at a volume ratio of 1:1. The solution still became turbid, but the precipitated solid powder was evenly dispersed in deionized water, and the fluorescence was still bright yellow; refer to Figure 1 .
[0040] Performance Testing
[0041] Reference Figure 2 , are transmission electron microscopy images of carbon dots prepared in Example 1, wherein Figure a is a TEM image of carbon dots obtained with acetic acid as solvent, from which it can be seen that the carbon dots are evenly distributed in a spherical shape, with a single particle diameter of about 5 nm; Figure b is a TEM image of carbon dots obtained with DMSO as solvent, from which it can be seen that, similar to that in acetic acid, the carbon dots are spherical, with a particle size of about 5 nm. Figures c and d correspond to the high-resolution transmission electron microscopy (HR-TEM) images of Figures a and b, respectively, from which it can be seen that when the solvents are acetic acid and DMSO, respectively, the fine lattice spacing of the carbon dots is 0.208 nm, with no obvious difference.
[0042] Reference Figure 3 , are the X-ray diffraction spectrum (a), Raman spectrum (b) and Fourier transform infrared spectrum (c) of the carbon dots prepared in Example 1; the X-ray diffraction (XRD) analysis results show that there is an obvious peak near 20°, which corresponds to the interplanar spacing shown in HR-TEM, indicating that there is a graphene-like structure in AIE-CDs. The Raman spectrum shows two peaks at 1340 and 1590 cm -1 The peaks represent the D peak and the G peak, which respectively describe the lattice defects of carbon atoms and the sp 2 The in-plane stretching vibration of the hybrid; I D / I G is 0.821, indicating that the sp 2 The content of graphite carbon atoms is relatively higher than that of disordered sp 3 Fourier transform infrared spectroscopy (FT-IR) confirmed the presence of functional groups or chemical bonds on the surface of carbon dots, including hydroxyl groups (3440 cm -1 ), amino (3100cm -1 ), amide carbonyl (1682cm -1 )、CN(1589cm -1 ) and C=C(1462cm -1 ) et al., proved that the prepared AIE-CDs contained nitrogen-containing functional groups.
[0043] Reference Figure 4, is the X-ray photoelectron diffraction spectrum (XPS) of the carbon dots prepared in Example 1. The peaks at 533.08, 284.8, 406.11, 200.1 and 164.35 eV belong to O1s, C 1s, N 1s, Yb 4d and Er 4d, respectively; the proportions of elements C, O, N, Yb and Er in AIE-CDs are 95.65%, 3.82%, 0.39%, 0.1% and 0.04%, respectively.
[0044] Reference Figure 5 , is the fluorescence spectrum of the carbon dots prepared in Example 1 at different excitation wavelengths. AIE-CDs has almost no detectable signal when in solution dispersion state, but exhibits yellow fluorescence when in powder aggregation state. When the excitation wavelength is between 300-440nm, the fluorescence signal gradually increases with the increase of the excitation wavelength. When the excitation wavelength is 440nm, the AIE-CDs aggregation state has the best imaging emission at 525; when the excitation wavelength increases further, the fluorescence signal drops sharply.
[0045] Reference Figure 6 , is an image of the carbon dots prepared in Example 1 on the cell nucleus. In order to study the distribution of AIE-CDs in Hela cells, the commercial organelle dye DAPI (a fluorescent dye that strongly binds to DNA and is specifically used for cell nucleus staining) and the commercial lysosome-specific dye Lyso-Tracker Green were used together with AIE-CDs to stain the cells. Figure 6 As shown in the figure, a, b, and c are the fluorescence images of AIE-CDs, DAPI, and Lyso-Tracker Green, respectively. DAPI dyes the Hela cell nucleus blue, Lyso-Tracker Green dyes the lysosome green, and AIE-CDs are also distributed in the cell nucleus and can dye the cell nucleus yellow. Figure d is the image after the AIE-CDs, DAPI, and Lyso-Tracker Green fluorescence images are superimposed, and the observation effect is more obvious.
[0046] Cell imaging method: HeLa cells were incubated in 2 mL of culture medium containing 10 μg / mL AIE-CDs solution for 30 min, then washed three times with PBS, and then further incubated with a commercial lysosome-specific probe (Lyso-Tracker Green, 100 nM) for 30 min, counterstained with 4% paraformaldehyde solution for 15 min, and the cell nuclei were stained with DAPI. The cell fluorescence was observed under a confocal laser scanning microscope (CLSM).
[0047] Reference Figure 7, are the imaging results of the carbon dots prepared in Example 1 on zebrafish embryos (Embruso) and larvae (Larvalzebranfish).
[0048] To verify the applicability of AIE-CDs for in vivo imaging, zebrafish embryos and larvae were used as vertebrate models because of their rapid embryonic development and the optical transparency of both embryos and larvae for imaging.
[0049] Zebrafish embryo imaging method: Use a disposable pipette to take 5 zebrafish or 5 zebrafish embryos, place them in a 6-well cell culture plate, add 2mL embryo culture medium containing 10μg / mL AIE-CDs solution, and incubate at 28℃ in the dark for 30 minutes. After the incubation, rinse the zebrafish or zebrafish embryos 3 times with PBS and then move them in. Heat the fixative solution to 85℃ in a metal bath until it melts, cool it down slightly (the cooling time is about 20 seconds, otherwise the temperature will cause the embryo to shrink if it is too high, and the viscosity will be too high if the temperature is too low, which is not conducive to adjusting the embryo position), take 500μL of fixative solution to the confocal culture dish, move the zebrafish or zebrafish embryo into the confocal culture dish, adjust the zebrafish to the appropriate position with a blunt needle under a stereo microscope, and observe the fluorescence of zebrafish or zebra embryo eggs under the field of view of a confocal laser scanning microscope (CLSM) after the fixative solution solidifies.
[0050] Reference Figure 7 In the imaging results, it can be seen in Figure c that fluorescence appears inside the embryo, but not in the yolk sac. AIE-CDs can enter the embryo through the chorion, and the difference in fluorescence intensity between the yolk sac and the internal area of the embryo shows that AIE-CDs have different degrees of affinity for different tissues of the embryo. In Figure f, the accumulation of AIE-CDs in the digestive system and yolk sac of zebrafish larvae is obvious, indicating that AIE-CDs enter the body of zebrafish larvae through ingestion and skin absorption, and also have tissue affinity for the larvae.
[0051] Example 2
[0052] This example provides the application of the aggregation-induced emission carbon dots prepared in Example 1 in cell imaging.
[0053] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A method for preparing aggregation-induced emission carbon dots, characterized in that: The following steps are involved: 1) dissolving tetraphenylethylene TPE, Er(NO3)3 and Yb(NO3)3 in glacial acetic acid and subjecting to ultrasonic treatment to obtain a mixture; 2) transferring the mixture obtained in step 1) into a reaction kettle and performing a hydrothermal reaction under heating; 3) After the reaction is completed, the mixture is cooled to room temperature, and deionized water is added to the obtained product to form a suspension; 4) After ultrasonic treatment of the suspension, centrifugation is performed to collect the solid product; the ultrasonic treatment and centrifugation steps are repeated, and the obtained solid product is vacuum dried to obtain aggregation-induced emission carbon dots; Step 1) is specifically as follows: 166-664 mg tetraphenylethylene TPE, 11.6-42.6 mg Er(NO3)3 and 65-260 mg Yb(NO3)3 are dissolved in 20-40 mL glacial acetic acid, and ultrasonically treated for 15-60 minutes to obtain a mixture.
2. The method for preparing aggregation-induced emission carbon dots according to claim 1, characterized in that: Step 1) is specifically as follows: 332 mg of tetraphenylethylene TPE, 21.3 mg of Er(NO3)3 and 129.2 mg of Yb(NO3)3 are dissolved in 40 mL of glacial acetic acid, and ultrasonically treated for 30 minutes to obtain a mixture.
3. The method for preparing aggregation-induced emission carbon dots according to claim 1, characterized in that: Step 2) is specifically as follows: the mixture obtained in step 1) is transferred to a reaction kettle and reacted at 170-200° C. for 8-24 hours.
4. The method for preparing aggregation-induced emission carbon dots according to claim 3, characterized in that: Step 2) is specifically as follows: the mixture obtained in step 1) is transferred into an 80 mL polytetrafluoroethylene-lined autoclave and reacted at 180° C. for 16 hours.
5. The method for preparing aggregation-induced emission carbon dots according to claim 1, characterized in that: Step 3) is specifically as follows: after the reaction is completed, the mixture is cooled to room temperature, and 200 mL of deionized water is added to the obtained product to form a suspension.
6. The method for preparing aggregation-induced emission carbon dots according to claim 1, characterized in that: Step 4) is specifically as follows: after ultrasonic treatment of the suspension for 2-10 minutes, centrifuge at a speed of 5000-20000 rpm for 5-20 minutes to collect the solid product; repeat the ultrasonic treatment and centrifugation steps 2-5 times, and vacuum dry the solid product at 50-70° C. to obtain aggregation-induced emission carbon dots.
7. The method for preparing aggregation-induced emission carbon dots according to claim 6, characterized in that: Step 4) is specifically as follows: after ultrasonic treatment of the suspension for 5 minutes, centrifugation at 10,000 rpm for 10 minutes was performed to collect the solid product; the ultrasonic treatment and centrifugation steps were repeated three times, and the solid product was vacuum dried at 60° C. to obtain aggregation-induced emission carbon dots.
8. An aggregation-induced emission carbon dot, characterized in that: It is prepared by the method described in any one of claims 1 to 7.
9. Use of the aggregation-induced emission carbon dots prepared by the method according to any one of claims 1 to 7 in cell imaging.