A zeolite molecular sieve supported platinum single atom cluster catalyst and its preparation method and application

By loading platinum single atom clusters on zeolite molecular sieve, uneven dispersion of precious metal catalysts and safety of activated carbon are solved, and efficient and environmentally friendly furfural reduction amination reaction is achieved, which improves the stability and selectivity of the catalyst and solves traditional tertiary amines. Problems of environmental pollution and insufficient activity of the synthesis process.

CN117160518BActive Publication Date: 2024-12-03NANJING TECH UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311123366.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-01
Publication Date
2024-12-03
Estimated Expiration
2043-09-01

AI Technical Summary

Technical Problem

Existing precious metal catalyst carriers such as activated carbon are prone to spontaneous combustion under dry air, which has problems with uneven dispersion and agglomeration of precious metals, resulting in a decrease in catalytic activity. The traditional tertiary amine synthesis process is seriously polluted and the catalyst activity and stability are poor.

Method used

The platinum single-atom cluster catalyst is loaded with zeolite molecular sieve. Through the strong adsorption of organic alkali and zeolite molecular sieve, the agglomeration of platinum is prevented and a high dispersion single-atom cluster is formed. It is used for furfural reduction amination reaction to achieve high efficiency, low cost and environmentally friendly. Tertiary amine synthesis.

Benefits of technology

It achieves high dispersion and high utilization of precious metals, excellent catalytic activity, long stability, low cost, and has high selectivity and high conversion in furfural reduction amination reaction, avoiding carbon deposits and easy separation and recovery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117160518B_ABST
    Figure CN117160518B_ABST
Patent Text Reader

Abstract

The present invention discloses a zeolite molecular sieve supported platinum single atom cluster catalyst and a preparation method thereof, wherein Pt in the catalyst is supported on a carrier as a cluster consisting of a single atom or multiple atoms; the preparation method is as follows: a quaternary ammonium base with a molecular weight of less than 300 is selected to prepare an organic alkaline solution, a zeolite molecular sieve is added to obtain a suspension, a platinum precursor solution is added to the suspension, and after continuous stirring at room temperature or under heating, solid-liquid separation is performed, and the obtained solid is ground, sieved, roasted, and reduced to obtain the catalyst. The preparation process of the method of the present invention is simple, and only one-pot method is required to synthesize the zeolite molecular sieve supported platinum single atom cluster catalyst; the catalyst is applied to the furfural reduction amination reaction, and the furfural conversion rate and the selectivity of the target product are both as high as more than 98%, the reaction route is simple and green, and the catalyst has high efficiency and good stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of precious metal catalysts, and relates to a zeolite molecular sieve-supported platinum catalyst, and in particular to a zeolite molecular sieve-supported platinum single atom cluster catalyst, a preparation method and an application thereof. Background Art

[0002] Single atom cluster catalyst is a new type of catalyst, which is composed of a cluster structure composed of a single atom or multiple atoms. Compared with traditional catalysts, single atom cluster catalysts have better catalytic performance and more stable catalytic effects, and are widely used in the fields of catalysis and materials.

[0003] The design of single-atom cluster catalysts is an extremely important process that determines the performance and effect of the catalyst. When designing single-atom cluster catalysts, many factors need to be considered, including the appropriate catalyst support, the composition and shape of the clusters, the interaction between the clusters and the support, and so on.

[0004] Most of the existing commercial precious metal catalyst carriers are activated carbon. Such catalyst products have high requirements for use conditions and are prone to spontaneous combustion in dry air, which poses potential safety risks. At the same time, such carriers have certain limitations on the dispersion and anchoring of precious metals, and precious metals are prone to agglomeration, which leads to a decrease in catalytic activity. Therefore, the development of a safe, stable, and highly catalytic new material has very important industrial application value.

[0005] Zeolite molecular sieve is a hydrated crystalline silicate with regular pore structure, high specific surface area, good thermal stability and mechanical strength. By utilizing its ion exchange characteristics, it can load different metals for specific catalytic reactions; by utilizing its specific pore shape and size, it can achieve shape-selective catalysis of certain raw materials or products; by utilizing its surface acid centers, it can be used for various reactions such as isomerization, disproportionation and alkylation.

[0006] Tertiary amines are a type of chemical intermediates that are closely related to daily life. They have important application value in the fields of cationic surfactants, fungicides and industrial additives. At present, the mainstream industrial manufacturing process starts from non-renewable fossil resources. The synthesis process represented by the chloroamination method has a long route, high raw material consumption, poor product quality, and a large amount of waste acid, which has caused serious environmental pollution and is gradually being eliminated. Therefore, exploring high-efficiency, low-cost, and environmentally friendly tertiary amine synthesis processes is of great significance to the realization of sustainable development strategies.

[0007] Furfural, as a commercialized biomass-based green chemical raw material (>250,000 tons / year), is regarded as a platform compound molecule that is one of the top chemicals "Top 10+4" derived from biomass. The reductive amination of furfural to prepare tertiary amines has attracted wide attention from academia and industry due to its high atom economy, simplicity and high efficiency. At present, the main problems of this reaction are still low catalyst activity and poor stability. Summary of the invention

[0008] The purpose of the present invention is to provide a zeolite molecular sieve supported platinum single atom cluster catalyst and a preparation method thereof, so as to solve the problem that Pt is difficult to disperse and easy to agglomerate in supported catalysts, and obtain a highly dispersed single atom cluster platinum catalyst.

[0009] Another object of the present invention is to provide an application of the catalyst in catalyzing the reductive amination reaction of furfural, which has the advantages of high furfural conversion rate, good selectivity, high catalyst activity and stability, a simple and reasonable reaction route, and realizes green and efficient manufacturing.

[0010] In order to achieve the above-mentioned invention object, the present invention adopts the following technical solutions:

[0011] The present invention provides a method for preparing a zeolite molecular sieve supported platinum single atom cluster catalyst, comprising the following steps:

[0012] (1) dissolving an organic base in a solvent to obtain an alkaline solution; the organic base is selected from one or more quaternary ammonium bases with a molecular weight of less than 300;

[0013] (2) adding the zeolite molecular sieve into the alkaline solution and stirring sufficiently to obtain a uniform suspension;

[0014] (3) adding the platinum precursor solution to the above suspension, stirring continuously at room temperature or under heating conditions, separating the solid and the liquid, washing, grinding the obtained solid, sieving and then roasting;

[0015] (4) The calcined product is subjected to a reduction treatment to obtain the zeolite molecular sieve-supported platinum single atom cluster catalyst.

[0016] In step (1), the organic base is preferably one or two of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, hexamethylammonium hydroxide and choline hydroxide.

[0017] The solvent is preferably one or more of methanol, ethanol, acetone, toluene, ethyl acetate, ethylene dichloride, and deionized water. When the solvent is a combination of two or more solvents, they need to be mutually soluble and not stratified.

[0018] Preferably, the pH of the alkaline solution is controlled at 8-11.

[0019] Furthermore, the topological structure of the zeolite molecular sieve described in step (2) includes any one of FAU, MFI, and BEA. For example, FAU type molecular sieves include X molecular sieves and Y molecular sieves, MFI type molecular sieves include Silicalite-1, ZSM-5, and TS-1 molecular sieves, and BEA type molecular sieves include Beta (β) molecular sieves.

[0020] Preferably, the zeolite molecular sieve is any one of TS-1, Silicalite-1, ZSM-5, β molecular sieve, and Y molecular sieve.

[0021] In step (3), the platinum precursor includes but is not limited to any one of chloroplatinic acid, sodium chloroplatinate, platinum nitrate, and tetraammine platinum nitrate.

[0022] Preferably, the platinum precursor solution is added dropwise to the suspension, stirred at room temperature for 20 to 60 minutes, and then heated to 60 to 85° C. and stirred for 60 to 120 minutes.

[0023] Preferably, the calcination temperature is 100-300° C. and the calcination time is 1-6 hours.

[0024] In step (4), the reduction treatment is carried out in a hydrogen atmosphere, preferably at 150 to 350° C. to reduce the prepared catalyst.

[0025] The present invention also provides a zeolite molecular sieve-loaded platinum single atom cluster catalyst prepared by the preparation method.

[0026] The catalyst uses zeolite molecular sieve as a carrier, and Pt is loaded on the carrier in the form of a single atom or a cluster composed of multiple atoms. Preferably, the single atom or cluster contains 1 to 25 platinum atoms.

[0027] Furthermore, the platinum content in the catalyst is 0.001%wt to 0.45%wt.

[0028] The present invention also provides the use of the zeolite molecular sieve supported single atom cluster catalyst in the reduction amination reaction of furfural, wherein the furfural also includes its derivatives, such as 5-methylfurfural and the like.

[0029] Furthermore, the catalyst is used as a catalyst for furfural reduction amination reaction, with furfural and dimethylamine as raw materials and H2 as a reducing agent; the raw materials furfural and dimethylamine, the above catalyst and solvent are added to a high-pressure reactor, hydrogen is introduced, and the temperature is raised to react with stirring, and the product N,N-dimethylfurfurylamine is obtained after reduction amination reaction.

[0030] Preferably, the temperature of the reductive amination reaction is 60-110° C., and the reaction time is 1-6 hours.

[0031] Preferably, the hydrogen pressure of the reductive amination is 0.1-3 MPa.

[0032] Preferably, the usage ratio of the zeolite molecular sieve supported single atom cluster catalyst to furfural is (100-350) g: (0.5-5) mol.

[0033] Furthermore, the solvent is one or more of deionized water, alcohol, ether, and alkane.

[0034] Preferably, the solvent is one or more of deionized water, methanol, ethanol, isopropanol, dioxane, tetrahydrofuran, and cyclohexane.

[0035] Beneficial effects: According to the preparation method of the zeolite molecular sieve supported single atom cluster catalyst of the present invention, the amount of precious metal used is small, the utilization rate is high, and the dispersibility is good; the Pt in the prepared catalyst is distributed in highly dispersed single atom clusters and has excellent catalytic activity. The preparation of the catalyst only requires a simple one-pot method, the process is simple, the repeatability is high, it is easy to scale up, and it is conducive to production.

[0036] The present invention adopts specific organic bases such as tetramethylammonium hydroxide and tetraethylammonium hydroxide in the preparation of the catalyst. Since the molecular sieve has certain acidity and the tetramethylammonium hydroxide and the like have alkalinity, they can produce strong adsorption effect with the carrier molecular sieve. At the same time, the organic base has a certain molecular size and occupies part of the steric hindrance, thereby providing a reliable site for the subsequent deposition and adsorption of the precious metal precursor. The molecular sieve carrier, the organic base and the platinum are closely combined to produce an electronic effect, thereby preventing the agglomeration of platinum and forming platinum nanocrystals.

[0037] In the catalyst prepared by the present invention, there is a strong interaction between the single atom cluster and the zeolite molecular sieve, the structure is stable, and the catalyst has a synergistic catalytic ability, high activity, utilization rate and stability of the precious metal, long service life, and low catalyst cost. The catalyst is applied to the reduction amination reaction of furfural. When the molecular sieve is used as a solid acid catalyst, it has a catalytic effect on the reduction amination reaction, can promote the adsorption and activation of aldehyde groups and amino groups, promote the coupling dehydration of aldehyde groups and amine groups, is beneficial to further hydrogenation reactions, and has high product selectivity; the zeolite molecular sieve-loaded single atom cluster catalyst of the present invention can catalyze the reduction amination reaction below 110°C and below 3MPa hydrogen pressure without generating carbon deposits; the zeolite molecular sieve-loaded single atom cluster catalyst of the present invention is easy to shape, easy to separate and recover, no loss of active metals, high utilization rate of precious metals, long service life, and low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is the XRD diagram of the Pt / Beta-1 reduced catalyst prepared by the present invention.

[0039] Figure 2 This is a spherical aberration corrected scanning transmission electron microscope photograph of the Pt / Beta-1 reduced catalyst prepared by the present invention.

[0040] Figure 3 It is the k-square weighted Fourier transform spectrum of the Pt L-edge of the Pt / Beta-1 reduced catalyst prepared by the present invention.

[0041] Figure 4 This is a high-resolution transmission electron microscopy photograph of the Pt / Beta-① catalyst prepared in Comparative Example 1.

[0042] Figure 5 This is a high-resolution transmission electron microscope photograph of the Pt / Beta-② catalyst prepared in Comparative Example 2. DETAILED DESCRIPTION

[0043] The specific embodiments of the present invention are described in detail below, but it should be pointed out that the protection scope of the present invention is not limited by these specific embodiments, but is determined by the claims.

[0044] Example 1

[0045] A zeolite molecular sieve supported platinum single atom cluster catalyst and preparation thereof, the steps are as follows:

[0046] 1) On a magnetic stirrer at a speed of 800 rpm, tetrapropylammonium hydroxide was added dropwise to a mixture of 600 ml of deionized water and methanol (volume ratio 5 / 1, the same below), stirred into a uniform solution and adjusted to pH = 10, and the temperature was controlled at 45 ° C for 30 min;

[0047] 2) Pour 20g of Beta molecular sieve into the above mixed solution and stir thoroughly;

[0048] 3) 4.9 ml of platinum nitrate solution (molar concentration of 0.025 mmol / ml) was added dropwise to the above mixture at a dropping speed of 1 s / drop, and the mixture was stirred for 30 min, then heated to 65 °C and stirred for 90 min;

[0049] 4) Stop heating, centrifuge, wash, and dry overnight at 80-85°C;

[0050] 5) Grind the obtained solid into powder and pass it through a 100-mesh sieve; roast it in an air atmosphere at 160°C for 3 hours (flow rate 50 ml / min, heating rate 1°C / min), and take it out after cooling to about 25°C;

[0051] 6) The sample obtained in step 5) is placed in a tubular furnace, hydrogen is introduced (flow rate 80 ml / min), and reduced at 180°C for 3 h (heating rate 1°C / min). After the tubular furnace is cooled to about 25°C, it is taken out and stored in a dry, oxygen-free environment to obtain a Beta molecular sieve-loaded platinum single atom cluster catalyst, denoted as Pt / Beta-1. The Pt content is determined by ICP to be 0.11% (wt%, the same below).

[0052] The XRD patterns and spherical aberration corrected scanning transmission electron micrographs of the obtained samples are shown in Figure 1 and Figure 2 As shown. Figure 1 It can be seen that the Pt / Beta-1 catalyst prepared by the present invention has BEA structural characteristic diffraction peaks at 2θ=7.8°, 22.6°, 27.01°, 29.32°, and 43.65°, indicating that the loading process of metal platinum does not destroy the topological structure of the beta molecular sieve. At the same time, there is no characteristic peak of the Pt(111) crystal plane near 39.7°. The surface-loaded platinum is very evenly dispersed on the molecular sieve. Figure 2 It can be seen that Pt on the molecular sieve appears in the form of single atomic dispersed clusters ( Figure 2 There are no metal crystals, and the single-atom clusters contain 1 to 25 platinum atoms.

[0053] Example 2

[0054] A zeolite molecular sieve supported platinum single atom cluster catalyst and preparation thereof, the steps are as follows:

[0055] 1) On a magnetic stirrer at a speed of 800 rpm, tetrabutylammonium hydroxide was added dropwise to 600 ml of a mixture of deionized water and methanol (4 / 1), stirred into a uniform solution and adjusted to pH = 10, and the temperature was controlled at 45 ° C for 30 min;

[0056] 2) Pour 20g of Beta molecular sieve into the above mixed solution and stir thoroughly;

[0057] 3) 9 ml of platinum nitrate solution (molar concentration of 0.04 mmol / ml) was added dropwise to the above mixture at a dropping speed of 1 s / drop, and the mixture was stirred for 30 min, then heated to 65 °C and stirred for 90 min;

[0058] 4) Stop heating, centrifuge, wash, and dry overnight at 80-85°C;

[0059] 5) Grind the obtained solid into powder and pass it through a 100-mesh sieve; roast it in an air atmosphere at 160°C for 3 hours (flow rate 50 ml / min, heating rate 1°C / min), and take it out after cooling to about 25°C;

[0060] 6) The sample obtained in step 5) was placed in a tubular furnace, hydrogen was introduced (flow rate 80 ml / min), and the sample was reduced at 180°C for 3 h (heating rate 1°C / min). After the tubular furnace was cooled to about 25°C, the sample was taken out and stored in a dry and oxygen-free environment to obtain a Beta molecular sieve-loaded platinum single atom cluster catalyst, denoted as Pt / Beta-2. The Pt content was determined by ICP to be 0.32%.

[0061] Example 3

[0062] A zeolite molecular sieve supported platinum single atom cluster catalyst and preparation thereof, the steps are as follows:

[0063] 1) On a magnetic stirrer at a speed of 800 rpm, add choline hydroxide dropwise into 600 ml of a mixture of deionized water and methanol (5 / 2), stir to form a uniform solution and adjust the pH to 10, and control the temperature at 45°C for 30 min;

[0064] 2) Pour 20g of Beta molecular sieve into the above mixed solution and stir thoroughly;

[0065] 3) 10 ml of platinum nitrate solution (molar concentration of 0.025 mmol / ml) was added dropwise to the above mixture at a dropping speed of 1 s / drop, and the mixture was stirred for 30 min, then heated to 65 °C and stirred for 90 min;

[0066] 4) Stop heating, centrifuge, wash, and dry overnight at 80-85°C;

[0067] 5) Grind the obtained solid into powder and pass it through a 100-mesh sieve; roast it in an air atmosphere at 160°C for 3 hours (flow rate 50 ml / min, heating rate 1°C / min), and take it out after cooling to about 25°C;

[0068] 6) The sample obtained in step 5) was placed in a tubular furnace, hydrogen was introduced (flow rate 80 ml / min), and the sample was reduced at 180°C for 3 h (heating rate 1°C / min). After the tubular furnace was cooled to about 25°C, the sample was taken out and stored in a dry and oxygen-free environment to obtain a Beta molecular sieve-loaded platinum single atom cluster catalyst, denoted as Pt / Beta-3. The Pt content was determined by ICP to be 0.24%.

[0069] Example 4

[0070] A zeolite molecular sieve supported platinum single atom cluster catalyst and preparation thereof, the steps are as follows:

[0071] 1) On a magnetic stirrer at a speed of 800 rpm, tetrapropylammonium hydroxide was added dropwise to 800 ml of a mixture of deionized water and ethanol (6 / 1), stirred into a uniform solution and adjusted to pH = 11, and the temperature was controlled at 45 ° C for 30 min;

[0072] 2) Pour 20g of Beta molecular sieve into the above mixed solution and stir thoroughly;

[0073] 3) 9 ml of sodium chloroplatinate solution (molar concentration of 0.05 mmol / ml) was added dropwise to the above mixture at a dropping speed of 2 s / 1 drop, and the mixture was stirred for 30 min, then heated to 85 °C and stirred for 60 min;

[0074] 4) Stop heating, centrifuge, wash, and dry overnight at 80-85°C;

[0075] 5) Grind the obtained solid into powder and pass it through a 100-mesh sieve; roast it in an air atmosphere at 250°C for 2h (flow rate 50ml / min, heating rate 1°C / min), and take it out after cooling to about 25°C;

[0076] 6) The sample obtained in step 5) was placed in a tubular furnace, hydrogen was introduced (flow rate 80 ml / min), and the sample was reduced at 280°C for 1 h (heating rate 1°C / min). After the tubular furnace was cooled to about 25°C, the sample was taken out and stored in a dry and oxygen-free environment to obtain a Beta molecular sieve-loaded platinum single atom cluster catalyst, denoted as Pt / Beta-4. The Pt content was determined by ICP to be 0.39%.

[0077] Example 5

[0078] A zeolite molecular sieve supported platinum single atom cluster catalyst and preparation thereof, the steps are as follows:

[0079] 1) On a magnetic stirrer at a speed of 800 rpm, choline hydroxide was added dropwise to 800 ml of a mixture of deionized water and ethanol (4 / 1), stirred into a uniform solution and adjusted to pH = 8, and the temperature was controlled at 45° C. for 30 min;

[0080] 2) Pour 20g of Beta molecular sieve into the above mixed solution and stir thoroughly;

[0081] 3) 5.6 ml of tetraammine platinum nitrate solution (molar concentration of 0.025 mmol / ml) was added dropwise to the above mixture at a dropping speed of 1 s / drop, and the mixture was stirred for 30 min, then heated to 75 °C and stirred for 90 min;

[0082] 4) Stop heating, centrifuge, wash, and dry overnight at 80-85°C;

[0083] 5) Grind the obtained solid into powder and pass it through a 100-mesh sieve; roast it in an air atmosphere at 200°C for 2h (flow rate 50ml / min, heating rate 1°C / min), and take it out after cooling to about 25°C;

[0084] 6) The sample obtained in step 5) was placed in a tubular furnace, hydrogen was introduced (flow rate 80 ml / min), and the sample was reduced at 200°C for 2 h (heating rate 1°C / min). After the tubular furnace was cooled to about 25°C, the sample was taken out and stored in a dry and oxygen-free environment to obtain a Beta molecular sieve-loaded platinum single atom cluster catalyst, denoted as Pt / Beta-5. The Pt content was determined by ICP to be 0.12%.

[0085] Example 6

[0086] A zeolite molecular sieve supported platinum single atom cluster catalyst and preparation thereof, the steps are as follows:

[0087] 1) On a magnetic stirrer at a speed of 800 rpm, tetraethylammonium hydroxide was added dropwise to 600 ml of a mixture of deionized water and methanol (5 / 1), stirred into a uniform solution and adjusted to pH = 10, and the temperature was controlled at 45°C for 30 minutes;

[0088] 2) Pour 20g ZSM-5 molecular sieve into the above mixed solution and stir thoroughly;

[0089] 3) 12 ml of tetraammine platinum nitrate solution (molar concentration of 0.025 mmol / ml) was added dropwise to the above mixture at a dropping speed of 1 s / drop, and the mixture was stirred for 30 min, then heated to 65 °C and stirred for 90 min;

[0090] 4) Stop heating, centrifuge, wash, and dry overnight at 80-85°C;

[0091] 5) Grind the obtained solid into powder and pass it through a 100-mesh sieve; roast it in an air atmosphere at 200°C for 2h (flow rate 50ml / min, heating rate 1°C / min), and take it out after cooling to about 25°C;

[0092] 6) The sample obtained in step 5) was placed in a tubular furnace, hydrogen was introduced (flow rate 80 ml / min), and the sample was reduced at 200°C for 2 h (heating rate 1°C / min). After the tubular furnace was cooled to about 25°C, the sample was taken out and stored in a dry and oxygen-free environment to obtain a ZSM-5 molecular sieve-loaded platinum single atom cluster catalyst, denoted as Pt / Z5. The Pt content was determined by ICP to be 0.27%.

[0093] Example 7

[0094] A zeolite molecular sieve supported platinum single atom cluster catalyst and preparation thereof, the steps are as follows:

[0095] 1) On a magnetic stirrer at a speed of 800 rpm, tetrapropylammonium hydroxide was added dropwise to 600 ml of a mixture of deionized water and ethanol (5 / 1), stirred into a uniform solution and adjusted to pH = 10, and the temperature was controlled at 45 ° C for 30 min;

[0096] 2) Pour 20g of Y molecular sieve into the above mixed solution and stir thoroughly;

[0097] 3) 14 ml of tetraammine platinum nitrate solution (molar concentration of 0.025 mmol / ml) was added dropwise to the above mixture at a dropping speed of 1 s / drop, stirred for 30 min, and then heated to 65 °C and stirred for 90 min;

[0098] 4) Stop heating, centrifuge, wash, and dry overnight at 80-85°C;

[0099] 5) Grind the obtained solid into powder and pass it through a 100-mesh sieve; roast it in an air atmosphere at 200°C for 2h (flow rate 50ml / min, heating rate 1°C / min), and take it out after cooling to about 25°C;

[0100] 6) The sample obtained in step 5) was placed in a tubular furnace, hydrogen was introduced (flow rate 80 ml / min), and the sample was reduced at 200°C for 2h (heating rate 1°C / min). After the tubular furnace was cooled to about 25°C, the sample was taken out and stored in a dry and oxygen-free environment to obtain a Y molecular sieve-supported platinum single atom cluster catalyst, denoted as Pt / Y. The Pt content was determined by ICP to be 0.31%.

[0101] Comparative Example 1

[0102] On a magnetic stirrer at a speed of 800 rpm, 20 g of Beta molecular sieve was poured into a mixture of 600 ml of deionized water and methanol, and then 10 ml of platinum nitrate solution (molar concentration of 0.025 mmol / ml) was added dropwise to the above mixture at a dropping speed of 1 s / 1 drop. The mixture was stirred thoroughly overnight and the solvent was then evaporated. The sample was dried at 110°C for 8 h, ground through a 100-mesh sieve, and calcined in a muffle furnace at 500°C for 3 h. The obtained sample was placed in a tubular furnace and introduced with hydrogen (flow rate of 80 ml / min), and reduced at 180°C for 2 h (heating rate of 1°C / min). The sample was taken out after the tubular furnace was cooled to about 25°C and stored in a dry, oxygen-free environment to obtain a Pt / Beta-① catalyst. The Pt content was 0.25% as determined by ICP.

[0103] Comparative Example 2

[0104] On a magnetic stirrer at a speed of 800 rpm, add sodium hydroxide aqueous solution (0.01 mmol / ml) dropwise into a 600 ml mixed solution of deionized water and methanol, stir evenly and adjust to pH = 10, and keep the temperature at 45 ° C for 30 min; pour 20 g of Beta molecular sieve into the above mixed solution and stir well; add 4.9 ml of platinum nitrate solution (molar concentration of 0.025 mmol / ml) dropwise into the above mixed solution at a dropping speed of 1 s / 1 drop, Stir thoroughly for 30 minutes, then heat to 65°C and continue stirring for 90 minutes; evaporate the solvent, dry the sample at 110°C for 8 hours, grind through a 100-mesh sieve, and calcine in a muffle furnace at 500°C for 3 hours. The obtained sample is placed in a tubular furnace, introduced with hydrogen (flow rate 80 ml / min), reduced at 200°C for 2 hours (heating rate 1°C / min), and taken out after the tubular furnace is cooled to about 25°C. It is stored in a dry, oxygen-free environment. The Pt content of the Pt / Beta-② catalyst determined by ICP is 0.11%.

[0105] Comparative Example 3

[0106] The Pt / Beta catalyst was prepared by the same method as in Example 1, except that in step (4), no centrifugal separation was performed. Instead, the temperature was raised to 90° C., the solvent was directly evaporated and dried to obtain a Pt / Beta-③ catalyst. The Pt content was determined by ICP to be 0.12%.

[0107] Example 8 Catalyst Performance Evaluation

[0108] Samples: Examples 1-7, Comparative Examples 1-3

[0109] Method: 200 mg of the reduced catalyst was placed in a high-pressure reactor, and 60 ml of ethanol, 4 mmol of furfural and 8 mmol of dimethylamine were added in sequence; after the reactor was installed, the reactor and the hydrogen cylinder were connected, and the air in the reactor was replaced with hydrogen three times to exhaust most of the air in the reactor; hydrogen was introduced to keep the hydrogen pressure in the reactor at 1.5 MPa; the temperature was adjusted to 90°C and maintained for 10 min. When the displayed temperature was within ±1°C of the set value, the stirring was turned on to 1000 rpm, and the reaction time lasted for 3 h; after the reaction was completed, the reactor was placed in an ice water bath and cooled to room temperature, 1.5 ml of the reaction solution was aspirated, and the catalyst was removed through a 0.25 μm filter head. The resulting clear liquid was quantitatively analyzed using a gas chromatograph (Agilent 8860). After separation using an HP-5 capillary column, the product was detected by a FID detector, and its conversion rate and yield were calculated using the internal standard method. The results are shown in Table 1.

[0110] Table 1 Catalytic activities of different catalysts in Examples 1 to 7 and Comparative Examples 1 to 3

[0111] Case catalyst Furfural conversion rate / % N, N-dimethylfurfurylamine yield / % Example 1 Pt / Beta-1 >99 98 Example 2 Pt / Beta-2 98 94 Example 3 Pt / Beta-3 98 95 Example 4 Pt / Beta-4 97 93 Example 5 Pt / Beta-5 >99 97 Example 6 Pt / Z5 >99 93 Example 7 Pt / Y 96 94 Comparative Example 1 Pt / Beta-① 47 15 Comparative Example 2 Pt / Beta-② 63 31 Comparative Example 3 Pt / Beta-③ 58 27

[0112] It can be seen from the results in Table 1 that, compared with the comparative samples Pt / Beta-①, Pt / Beta-② and Pt / Beta-③, the catalysts prepared according to the method of the present invention all exhibit excellent catalytic activity (conversion rate) and target product yield. The reason for the excellent performance is closely related to the platinum structure on the catalyst.

[0113] The catalysts obtained by conventional loading methods, such as Pt / Beta-① and Pt / Beta-②, have certain limitations in the dispersion of precious metals, the Pt particles are large, and are very easy to agglomerate. Figure 4 and Figure 5 The high-resolution transmission electron microscopy photos of Pt / Beta-① and Pt / Beta-② show obvious platinum nanoparticles (shown as black dots in the figure), and the average size is about 4.5 nanometers. As mentioned above, the spherical aberration-corrected scanning transmission electron microscopy photos of the Pt / Beta-1 sample prepared by the present invention show that Pt on the molecular sieve is in the form of single-atom dispersed clusters, and there are no metal crystals. The k-square weighted Fourier transform spectroscopy characterization test of the L edge of Pt is further adopted. Figure 3 Zhongzai The strong peak at is attributed to the characteristic peak of metal platinum (Pt-foil). The strong peak at is attributed to the characteristic peak of platinum oxide (PtO2). The main peak intensity of Pt in the Pt / Beta-1 sample prepared by the present invention is There is almost no The peak at , indicates that the coordination state of Pt in the catalyst prepared by the present invention is mainly Pt-O, and there is no platinum nano-metal crystal, which is consistent with the structure characterized by electron microscopy. This structural difference is the main reason for the excellent performance of the catalyst of the present invention.

[0114] Example 9

[0115] The Pt / Beta-1 prepared in Example 1 was used as a catalyst for the reductive amination reaction of furfural and dimethylamine, H2 was used as a reducing agent, raw materials furfural and dimethylamine, a catalyst and a solvent were added to a high-pressure reactor, hydrogen was introduced, and the temperature was raised to react with stirring, and the product N,N-dimethylfurfurylamine was obtained after the reductive amination reaction. The method of Example 8 was specifically referred to, wherein the reaction pressures were 0.1, 0.5 and 1 MPa of hydrogen, respectively, and the results are shown in Table 2.

[0116] Table 2 Catalytic activity data of the catalyst in Example 1 for the reductive amination reaction of furfural under different hydrogen pressures

[0117] serial number catalyst Reaction pressure / MPa Furfural conversion rate / % N, N-dimethylfurfurylamine yield / % 1 Pt / Beta-1 0.1 13 11 2 Pt / Beta-1 0.5 58 57 3 Pt / Beta-1 1.0 83 82 4 Pt / Beta-1 1.5 >99 98

[0118] As shown in Table 2, in the furfural reduction amination reaction of the Pt / Beta-1 catalyst prepared in Example 1, as the hydrogen pressure increases, the furfural conversion rate and the yield of dimethylfurfurylamine increase accordingly, and the selectivity (yield divided by conversion rate) does not change significantly, and the higher the reaction pressure, the easier the reaction occurs. The zeolite molecular sieve supported single atom cluster catalyst of the present invention, the furfural conversion rate and the yield of dimethylfurfurylamine in the catalytic reduction amination reaction reach more than 80% under 90°C and 1.0MPa hydrogen pressure, and both reach more than 98% under 1.5MPa hydrogen pressure.

[0119] Example 10 Cyclic stability test:

[0120] The stability of Pt / Beta-1 prepared in Example 1 was tested as follows:

[0121] The reaction liquid after the catalyst participated in the performance test was collected, and the catalyst was separated by centrifugation. The catalyst was then put into use for the second time without any treatment. The same reaction steps as in Example 8 were adopted to carry out the catalytic reduction amination reaction of furfural and dimethylamine. The operation was repeated 4 times. The experimental results are shown in Table 3.

[0122] Table 3 Experimental results of recycling of catalyst in Example 1

[0123] serial number Use times Furfural conversion rate / % N, N-dimethylfurfurylamine yield / % 1 1 >99 98 2 2 >99 98 3 3 >99 97 4 4 >99 97

[0124] From the recycling results in Table 3, it can be seen that the Pt / Beta-1 catalyst is easy to separate and recycle, has good recycling availability and stability, the catalyst still has good catalytic performance after being used 4 times, and the conversion rate of furfural is more than 99%, so the single atom cluster catalyst Pt / Beta-1 of the present invention has good recycling repeatability.

Claims

1. A method for preparing a zeolite molecular sieve supported platinum single atom cluster catalyst, comprising the following steps: (1) dissolving an organic base in a solvent to obtain an alkaline solution; the organic base is selected from one or more quaternary ammonium bases with a molecular weight of less than 300; (2) adding the zeolite molecular sieve into the alkaline solution and stirring thoroughly to obtain a uniform suspension; (3) Add the precious metal platinum precursor solution to the above suspension, stir at room temperature for 20 to 60 minutes, then heat to 60 to 85°C and continue stirring for 60 to 120 minutes, separate the solid and liquid, wash, grind the obtained solid, sieve and then roast; (4) The calcined product obtained in step (3) is subjected to a reduction treatment to obtain the zeolite molecular sieve-supported platinum single atom cluster catalyst.

2. The preparation method according to claim 1, characterized in that: In step (1), the organic base is one or more of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, hexamethylammonium hydroxide, and choline hydroxide.

3. The preparation method according to claim 1, characterized in that: In step (1), the solvent is one or more of methanol, ethanol, acetone, toluene, ethyl acetate, dichloroethane, and deionized water.

4. The preparation method according to claim 1, characterized in that: In step (2), the topological structure of the zeolite molecular sieve is any one of FAU, MFI and BEA.

5. The preparation method according to claim 1, characterized in that: In step (3), the precursor is any one of chloroplatinic acid, sodium chloroplatinate, platinum nitrate, and tetraammine platinum nitrate.

6. The preparation method according to claim 1, characterized in that: In step (3), the calcination temperature is 100 to 300° C. and the calcination time is 1 to 6 hours.

7. The preparation method according to claim 1, characterized in that: In step (4), the reduction treatment is carried out at 150-350° C. in a hydrogen atmosphere.

8. The zeolite molecular sieve supported platinum single atom cluster catalyst prepared by the preparation method according to any one of claims 1 to 7.

9. The zeolite molecular sieve supported platinum single atom cluster catalyst according to claim 8, characterized in that: The platinum content in the catalyst is 0.001%wt to 0.45%wt.

10. Use of the zeolite molecular sieve supported platinum single atom cluster catalyst according to claim 8 in the reductive amination reaction of furfural.

Citation Information

Patent Citations

  • Preparation method of monatomic molding catalyst with uniform crystal phase

    CN115739169A

  • Application of supported catalyst in preparation of furfuryl amine by catalyzing reductive amination of furfural

    CN116272966A