A kind of ultra-high performance mass concrete with low hydration heat and preparation method thereof

Through the combination of AlN-silicon aluminum microporous aggregate and low-melting fiber modified steel fiber, the high hydration heat and high shrinkage problems of ultra-high performance concrete in large-volume components are solved, and the mechanical properties and thermal insulation are improved The temperature rise is reduced, suitable for a wide range of applications.

CN117164297BActive Publication Date: 2024-11-12HUAXIN CEMENT CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311002454.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-10
Publication Date
2024-11-12
Estimated Expiration
2043-08-10

AI Technical Summary

Technical Problem

The application of ultra-high performance concrete in large volume components is limited by high hydration heat and high shrinkage risks, and the prior art is difficult to reduce hydration heat and improve mechanical properties at the same time.

Method used

AlN-silicon aluminum microporous aggregate and low melting point fiber modified steel fiber are used to prepare microporous aggregate and modified steel fiber through high-temperature reaction, reducing the adiabatic temperature rise and shrinkage of concrete, while improving the mechanical properties of concrete .

Benefits of technology

The adiabatic temperature rise is reduced to below 70℃, the self-shrinkage and dry shrinkage of 180d are significantly reduced, the compressive strength of 28d reaches above 180MPa, and the flexural strength reaches above 26MPa, which significantly improves the mechanical properties and durability of ultra-high performance large-volume concrete. performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004386772860000081
    Figure BDA0004386772860000081
  • Figure HDA0004386772870000011
    Figure HDA0004386772870000011
Patent Text Reader

Abstract

The present invention discloses a low hydration heat ultra-high performance mass concrete, which includes the following components by weight: 640-750 parts of cement, 90-110 parts of low-quality silica fume, 105-150 parts of ultrafine mineral powder, 75-106 parts of fly ash micro-beads, 900 parts of AlN-silicon-aluminum microporous aggregate, 204-234 parts of water, 8.5-12.8 parts of polycarboxylic acid water reducer, and low-melting fiber modified steel fiber accounting for 2-3% of the volume of mass concrete; wherein, AlN-silicon-aluminum microporous aggregate is made of kaolin, low-quality silica fume, α-Al2O3 micro-powder, AlN-waste rubber powder-based powder as main raw materials, mixed with water, and then obtained by molding, calcining, crushing and screening. The present invention can significantly improve the mechanical properties of ultra-high performance mass concrete and reduce shrinkage while effectively reducing the hydration heat of ultra-high performance mass concrete, and is suitable for promotion and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and specifically relates to a low hydration heat ultra-high performance concrete and a preparation method thereof. Background Art

[0002] Ultra-high performance concrete is increasingly used in beam-slab-column structures, thin-wall structures, thin-shell structures, repair and reinforcement and other fields due to its excellent working performance, mechanical properties and durability. However, the amount of adhesive used in ultra-high performance concrete is much higher than that in ordinary mass concrete (about 2-3 times the amount of adhesive used in ordinary mass concrete), and ultra-high performance concrete usually requires the use of highly active mineral admixtures and high-strength grade cement. At the same time, coarse aggregate needs to be removed and fine sand needs to be used for preparation, resulting in its hydration heat being much higher than that of ordinary mass concrete. The hydration adiabatic temperature rise of ultra-high performance concrete can reach above 95°C, while the hydration adiabatic temperature rise of ordinary mass concrete is usually below 75°C, which makes the risk of cracking of mass concrete prepared with ultra-high performance concrete higher, limiting its application in large-volume components.

[0003] At present, there are some studies on the hydration heat of ultra-high performance concrete with low hydration heat, such as: Patent CN114133177A discloses a low-carbon C130-C140 ultra-high performance self-compacting concrete containing coarse aggregate, which regulates the hydration heat of cementitious materials based on the technology of large-volume fly ash microspheres, and proposes a low-heat cementitious system, so that the adiabatic temperature rise of concrete is no more than 67°C, which is about 13-20°C lower than that of the same-grade UHPC. Although this patent can effectively reduce the adiabatic temperature rise of concrete, the use of large-volume fly ash microspheres limits the improvement of the mechanical properties of ultra-high performance concrete (28-day compressive strength is less than 150MPa); in addition, although the coarse aggregate used can reduce the shrinkage of concrete, it also increases the interface transition zone between the slurry and the aggregate, resulting in the toughness of the prepared ultra-high performance concrete being lower than that of the ultra-high performance concrete without coarse aggregate. Summary of the invention

[0004] The main purpose of the present invention is to provide a low hydration heat ultra-high performance mass concrete in response to the problems and shortcomings of the prior art. While effectively reducing the hydration heat of the ultra-high performance mass concrete, the present invention can greatly improve the mechanical properties of the ultra-high performance mass concrete and reduce shrinkage, etc., and is suitable for promotion and application.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] A low hydration heat ultra-high performance mass concrete comprises the following components by weight: 640-750 parts of cement, 90-110 parts of low-quality silica fume, 105-150 parts of ultrafine mineral powder, 75-106 parts of fly ash micro-beads, 900 parts of AlN-silica-alumina microporous aggregate, 204-234 parts of water, 8.5-12.8 parts of polycarboxylic acid water reducer, and low-melting-point fiber-modified steel fiber accounting for 2-3% of the volume of the low hydration heat ultra-high performance mass concrete; wherein the AlN-silica-alumina microporous aggregate is prepared from kaolin, low-quality silica fume, α-Al2O3 micro-powder, and AlN-waste rubber powder-based powder as main raw materials, which are mixed with water, and then obtained by filter pressing, drying, calcining, crushing, and screening.

[0007] Optionally, the mass ratio of the kaolin, low-quality silica fume, α-Al2O3 micropowder, and AlN-waste rubber powder-based powder is 1:(0.3-0.5):(0.08-0.1):(0.24-0.3).

[0008] Optionally, the AlN-waste rubber powder-based powder is obtained by placing a uniform mixture of waste rubber powder and α-Al2O3 powder in a nitrogen atmosphere for high-temperature reaction; wherein the α-Al2O3 powder accounts for 5-10% of the mass of the waste rubber powder.

[0009] Optionally, the waste rubber powder is a powder with a particle size of 100-200 mesh obtained by crushing and grinding discarded tires.

[0010] Optionally, the high temperature reaction is carried out at a temperature of 800-900°C for 1-2 hours and a heating rate of 5-10°C / min.

[0011] Optionally, in the step of adding water and mixing, water is added until the moisture content of the obtained mixture is 12-15%.

[0012] Optionally, the temperature used in the drying step is 105-110°C.

[0013] Optionally, the calcination temperature is 1200-1350° C., the time is 1-2 h, and the heating rate is 5-10° C. / min.

[0014] Optionally, the screening step obtains AlN-silicate-alumina microporous aggregate with a particle size of 0-1 mm and 1-3 mm, wherein the water absorption rate of the AlN-silicate-alumina microporous aggregate is 3.5-5.5%.

[0015] Furthermore, the mass ratio of the aggregate with a particle size of 0-1 mm to the aggregate with a particle size of 1-3 mm in the AlN-silicon-alumina microporous aggregate is 1:(0.6-1).

[0016] The present invention uses kaolin as a raw material. As the calcination temperature increases, when the calcination temperature rises to above 400°C, the kaolinite therein begins to undergo a dehydration reaction. When the temperature continues to rise to above 980°C, the kaolinite begins to undergo a phase change and is converted into mullite accompanied by the generation of silicon dioxide. When the temperature continues to rise to above 1200°C, the silicon dioxide decomposed by the kaolinite mullite, the silicon dioxide in the low-quality silica ash and the α-Al2O3 micropowder react to generate mullite. In the process of forming mullite, the carbon black in the waste rubber powder that has not reacted completely and the ash in the low-quality silica ash are oxidized to form a gas encapsulated in the molten liquid phase. In the process of preparing ultra-high performance large-volume concrete, micropores of 20-50 nm are formed, and the relatively stable inorganic fillers in the waste rubber powder and the AlN formed by the high-temperature reaction are dispersed in the molten liquid phase to form a solid pore wall, so that the prepared AlN-silicon-aluminum microporous aggregate has micropores and high parent rock strength; the AlN-silicon-aluminum microporous aggregate with a microporous structure has an internal curing effect when preparing ultra-high performance large-volume concrete, which can greatly reduce shrinkage. At the same time, the AlN in the AlN-silicon-aluminum microporous aggregate has a good thermal conductivity, which can quickly transfer the heat inside the concrete to the outside and reduce the temperature inside the concrete.

[0017] Optionally, the low-melting point fiber modified steel fiber is formed by spraying molten low-melting point fiber onto the surface of the steel fiber, wherein the diameter of the steel fiber is 0.18-0.22 mm, the length is 13-15 mm; the aspect ratio is 60-70; and the average spray thickness of the low-melting point fiber on the surface of the steel fiber is 0.05-0.1 mm.

[0018] Furthermore, before the molten low-melting point fiber is hardened, quartz sand of 120-200 mesh is sprinkled into the steel fiber surface sprayed with the low-melting point fiber so that a layer of quartz sand is bonded to the surface of the steel fiber, wherein the bonding amount of the quartz sand is 7.0-9.0% of the mass of the steel fiber.

[0019] Optionally, the low-melting-point fiber has a melting point of 50-95°C.

[0020] In the above scheme, the low melting point fiber can be selected from water-soluble low melting point explosion-proof fiber and the like.

[0021] Optionally, the low melting point fiber is sprayed onto the surface of the steel fiber in layers in sequence according to the melting point temperature gradient of 90-95°C, 70-75°C, and 50-60°C to obtain low melting point fiber modified steel fiber.

[0022] The present invention modifies the steel fiber by low-melting point fiber. As the temperature inside the concrete increases, when the melting point of the low-melting point fiber is reached, it begins to absorb heat and melt, thereby effectively reducing the temperature inside the concrete. At the same time, the quartz sand bonded to the surface of the low-melting point fiber falls off as the low-melting point fiber melts. The fallen quartz sand can be filled in the weak area formed between the steel fiber and the slurry due to the melting of the low-melting point fiber, further effectively alleviating some of the negative effects caused by the melting of the low-melting point fiber, and ensuring that the obtained low-hydration heat ultra-high performance large-volume concrete has higher strength. In addition, the low-melting point fiber is further set to a gradient of melting point temperature according to the cement hydration exothermic process, which is conducive to effectively controlling the temperature reduction rate of the entire hydration process, avoiding too fast a cooling rate, causing temperature stress inside the concrete, and causing problems such as deformation or cracks in the concrete structure.

[0023] Optionally, the cement is ordinary Portland cement or Portland cement with a grade of 42.5 or above.

[0024] Optionally, the low-quality silica ash has an ash content of ≥4.5wt%, a silicon dioxide content of <85wt%, a water demand ratio of >130%, and a 28d compressive activity index of <85%.

[0025] Optionally, the particle size of the ultrafine mineral powder is ≥325 mesh.

[0026] Optionally, the fly ash microspheres have a water demand ratio of ≤95% and a 28d compressive activity index of ≥110%.

[0027] Optionally, the steel fiber has a diameter of 0.18-0.22 mm, a length of 13-15 mm, and an aspect ratio of 60-70.

[0028] Optionally, the water reduction rate of the polycarboxylate water-reducing agent is ≥25%.

[0029] The method for preparing the above-mentioned low hydration heat ultra-high performance large volume concrete comprises the following steps:

[0030] 1) Mix the weighed cement, low-quality silica fume, ultrafine mineral powder and fly ash microbeads evenly (1-2 minutes) to obtain mixture A;

[0031] 2) Take 20-30% of the mixed material A, add water thereto, stir evenly (1.5-2.5 minutes), add AlN-silicon-alumina microporous aggregate, continue to stir evenly (1-2 minutes), and obtain the slurry-coated AlN-silicon-alumina microporous aggregate mixture B;

[0032] 3) Add the remaining mixture A and the polycarboxylate water-reducing agent to the obtained AlN-silicon-alumina microporous aggregate mixture B, and stir evenly (2-3 minutes) to obtain a mixture C;

[0033] 4) Add low-melting-point fiber-modified steel fiber to the obtained mixture C, and stir evenly (1-2 minutes) to obtain the low-hydration heat ultra-high performance large-volume concrete.

[0034] The low hydration heat ultra-high performance large volume concrete prepared according to the above scheme has an adiabatic temperature rise of less than 70°C (can be as low as 65°C), a 7d autogenous shrinkage of less than 310με (can be as low as 210με), a 180d shrinkage of less than 160με (can be as low as 108με), a 28d compressive strength of more than 180MPa (can be as high as 217MPa), and a flexural strength of more than 26MPa (can be as high as 37MPa).

[0035] After mixing the powders, the present invention first takes part of the mixture and stirs it into slurry, and pre-coats the AlN-silicon-aluminum microporous aggregate. The slurry is adsorbed in the micropores on the surface of the AlN-silicon-aluminum microporous aggregate, which can slow down the adsorption rate and release rate of free water in the slurry, thereby reducing the influence of the slurry on the fluidity of the slurry; and as the cement hydration proceeds, the water adsorbed in the AlN-silicon-aluminum microporous aggregate is slowly released due to the coating, thereby reducing the cement hydration rate, delaying the hydration process, and further reducing the adiabatic temperature rise of the prepared ultra-high performance large-volume concrete, and at the same time, the risk of shrinkage cracking is effectively reduced in conjunction with the effect of its internal curing.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] 1. The present invention adopts a method of coordinating multiple technologies such as internal curing, high thermal conductivity, and high heat absorption, and takes the most compact stacking principle as the theoretical basis. It adopts self-made AlN-silicon aluminum microporous aggregate and low melting point fiber modified steel fiber to cooperate with each other, which can effectively reduce the hydration heat of ultra-high performance mass concrete, greatly improve the mechanical properties of ultra-high performance mass concrete, and reduce shrinkage;

[0038] 2. The present invention adopts low-quality silica fume to replace the existing commonly used high-quality silica fume, breaking the concept of improving the strength by reducing the water-binder ratio when preparing the existing ultra-high performance concrete, and increasing the water-binder ratio of the system to 0.20-0.23. At the same time, highly active ultra-fine mineral powder and homemade AlN-silicon-alumina microporous aggregate are used to effectively make up for the deficiencies of low-quality silica fume in activity and large water demand, while ensuring that the obtained ultra-high performance large-volume concrete has high strength while taking into account good working performance; in addition, the low-quality silica fume used can effectively reduce the preparation cost of ultra-high performance large-volume concrete, and provide direction for the application of low-quality silica fume in ultra-high performance concrete. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The hydration temperature rise diagram of the ultra-high performance concrete obtained in Examples 2, 3 and Comparative Example 2. DETAILED DESCRIPTION

[0040] The technical solution of the present invention is further described below through specific implementation methods. To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows.

[0041] The raw material indicators used in each embodiment of the present invention are as follows:

[0042] The cement is ordinary Portland cement of grade P·O52.5;

[0043] The ash content of low-quality silica fume is 10.5%, the silicon dioxide content is 78%, its 28d compressive activity index is 80%, and the water requirement ratio is 138%;

[0044] The particle size of the ultrafine mineral powder is 325 mesh, its 28d compressive activity index is 119%, and its water requirement ratio is 98%;

[0045] The water demand ratio of fly ash microspheres is 91%, and the 28d compressive activity index is 112%;

[0046] The average diameter of the steel fiber is 0.20 mm, the average length is 14 mm, and the average aspect ratio is 70;

[0047] The water reduction rate of polycarboxylate water reducer is 25%.

[0048] The waste rubber powder used is a powder with a particle size of 100-200 mesh obtained by crushing and grinding discarded tires.

[0049] The low-melting-point fibers with melting points of 50° C., 75° C., and 95° C. are commercially available water-soluble low-melting-point explosion-proof fibers.

[0050] The quartz sand used in the comparative example is 40-70 mesh quartz sand.

[0051] Example 1

[0052] A low hydration heat ultra-high performance mass concrete, comprising the following components by weight: 640 parts of cement, 90 parts of low-quality silica fume, 150 parts of ultra-fine mineral powder, 75 parts of fly ash micro-beads, 900 parts of AlN-silicon-alumina microporous aggregate, 212 parts of water, 11.3 parts of polycarboxylic acid water reducer, and low-melting-point fiber-modified steel fiber accounting for 3% of the volume of the low hydration heat ultra-high performance mass concrete; the water-binder ratio used is 0.22;

[0053] The AlN-silicon-alumina microporous aggregate is prepared by the following method: adding α-Al2O3 powder (accounting for 8% of the mass of the waste rubber powder) to the waste rubber powder, mixing evenly, heating to 800°C in a nitrogen atmosphere at a heating rate of 10°C / min for 2h to obtain the AlN-waste rubber powder-based powder; mixing kaolin, low-quality silica fume, α-Al2O3 powder, and AlN-waste rubber powder-based powder in a mass ratio of 1:0.4:0.1:0.28, adding a certain amount of water, stirring evenly, and mixing the mixture. The moisture content of the mixture is 12% to obtain AlN-silicon-aluminum microporous raw material; after the AlN-silicon-aluminum microporous raw material is filter-pressed and formed, it is dried at 105°C, then heated to 1200°C at a heating rate of 10°C / min, calcined for 2 hours, and cooled to obtain AlN-silicon-aluminum microporous clinker, and the Mohs hardness of the obtained AlN-silicon-aluminum microporous clinker is between 8 and 9; the AlN-silicon-aluminum microporous clinker is crushed and sieved to obtain 0-1mm and 1-3mm AlN-silicon-aluminum microporous aggregates, wherein the water absorption rate of the 0-1mm AlN-silicon-aluminum microporous aggregate is 3.52%, and the water absorption rate of the 1-3mm AlN-silicon-aluminum microporous aggregate is 5.05%.

[0054] The low-melting-point fiber-modified steel fiber is prepared by the following method: low-melting-point fiber with a melting point temperature of 75° C. is melted and then sprayed onto the surface of the steel fiber to obtain the low-melting-point fiber-modified steel fiber, wherein the average spraying thickness is 0.05 mm;

[0055] The low hydration heat ultra-high performance mass concrete is prepared by the following method:

[0056] According to the above raw material ratio, the weighed cement, low-quality silica fume, ultrafine mineral powder, and fly ash microbeads are mixed for 2 minutes to obtain mixture A; 20% of mixture A is taken, and the water in the above raw material ratio is added, and after stirring for 1.5 minutes, AlN-silica-alumina microporous aggregate is added, and stirring is continued for 2 minutes to obtain a slurry-coated AlN-silica-alumina microporous aggregate mixture B, wherein the AlN-silica-alumina microporous aggregate is composed of 0-1mm and 1-3mm particle sizes in a mass ratio of 1:1; the remaining mixture A and polycarboxylate water-reducing agent are added to the slurry-coated AlN-silica-alumina microporous aggregate mixture B, and the mixture is stirred for 3 minutes to obtain a mixture C; low-melting-point fiber-modified steel fiber is added to the mixture C, and the mixture is stirred for 1 minute to obtain low hydration heat ultra-high performance large-volume concrete.

[0057] Example 2

[0058] A low hydration heat ultra-high performance large volume concrete, the preparation method of which is substantially the same as that of Example 1, except that the components and their weight proportions are: 750 parts of cement, 90 parts of low-quality silica fume, 105 parts of ultrafine mineral powder, 75 parts of fly ash microspheres, 900 parts of AlN-silica-alumina microporous aggregate, 204 parts of water, 11.3 parts of polycarboxylic acid water reducer, and low-melting-point fiber-modified steel fiber accounting for 3% of the volume of the low hydration heat ultra-high performance large volume concrete; the water-cement ratio adopted is 0.2.

[0059] Example 3

[0060] A low hydration heat ultra-high performance mass concrete, the preparation method of which is substantially the same as that of Example 1, except that:

[0061] 1) The components and their weight proportions are: 750 parts of cement, 90 parts of low-quality silica fume, 105 parts of ultrafine mineral powder, 75 parts of fly ash microspheres, 900 parts of AlN-silicon-alumina microporous aggregate, 204 parts of water, 11.3 parts of polycarboxylate water reducer, and low-melting-point fiber-modified steel fiber accounting for 3% of the volume of low-hydration heat ultra-high performance mass concrete; the water-binder ratio used is 0.2;

[0062] 2) The preparation steps of low-melting point fiber modified steel fiber include: melting low-melting point fibers with melting points of 95°C, 75°C, and 50°C, and spraying them onto the surface of steel fibers in layers in sequence according to a melting point temperature gradient of 95°C, 75°C, and 50°C to obtain low-melting point fiber modified steel fiber, wherein the total average spraying thickness is 0.1 mm, and the spraying thickness of each layer is the same.

[0063] Example 4

[0064] A low hydration heat ultra-high performance large volume concrete, the preparation method of which is substantially the same as that of Example 1, except that the components and their weight proportions are: 700 parts of cement, 110 parts of low-quality silica fume, 130 parts of ultrafine mineral powder, 106 parts of fly ash microspheres, 900 parts of AlN-silica-alumina microporous aggregate, 234 parts of water, 12.8 parts of polycarboxylic acid water reducer, and low-melting-point fiber-modified steel fiber accounting for 3% of the volume of the low hydration heat ultra-high performance large volume concrete; the water-cement ratio adopted is 0.22.

[0065] Example 5

[0066] A low hydration heat ultra-high performance large volume concrete, the preparation method of which is substantially the same as that of Example 1, except that the components and their weight proportions are: 640 parts of cement, 100 parts of low-quality silica fume, 150 parts of ultrafine mineral powder, 95 parts of fly ash microspheres, 900 parts of AlN-silica-alumina microporous aggregate, 220 parts of water, 8.5 parts of polycarboxylic acid water reducer, and low-melting-point fiber-modified steel fiber accounting for 3% of the volume of the low hydration heat ultra-high performance large volume concrete; the water-cement ratio adopted is 0.22.

[0067] Example 6

[0068] A low hydration heat ultra-high performance mass concrete, the preparation method of which is substantially the same as that of Example 1, except that:

[0069] 1) The components and their weight proportions are: 640 parts of cement, 100 parts of low-quality silica fume, 150 parts of ultrafine mineral powder, 95 parts of fly ash microspheres, 900 parts of AlN-silicon-alumina microporous aggregate, 220 parts of water, 8.5 parts of polycarboxylate water reducer, and low-melting-point fiber-modified steel fiber accounting for 3% of the volume of low-hydration heat ultra-high performance mass concrete; the water-binder ratio used is 0.22;

[0070] 2) The preparation method of low-melting-point fiber modified steel fiber includes the following steps: melting the low-melting-point fiber with a melting point temperature of 75°C and spraying it onto the surface of the steel fiber, wherein the average spraying thickness is 0.05 mm, and before the molten low-melting-point fiber hardens, 120-200 mesh quartz sand is sprinkled into it, so that a layer of quartz sand is bonded to the surface of the steel fiber sprayed with the low-melting-point fiber, wherein the bonding amount of quartz sand is 7.8% of the mass of the steel fiber, thereby obtaining low-melting-point fiber modified steel fiber.

[0071] Example 7

[0072] A low hydration heat ultra-high performance large volume concrete, the preparation method of which is substantially the same as that of Example 6, except that the volumetric dosage of the low melting point fiber modified steel fiber is 2%.

[0073] Comparative Example 1

[0074] An ultra-high performance concrete comprises the following components by weight: 750 parts of cement, 90 parts of low-quality silica fume, 105 parts of ultra-fine mineral powder, 75 parts of fly ash microspheres, 900 parts of quartz sand, 184 parts of water, 11.3 parts of polycarboxylate water reducer, and steel fiber accounting for 3% of the volume of the ultra-high performance concrete; the water-cement ratio used is 0.18;

[0075] The method specifically includes the following preparation steps: evenly mixing the weighed cement, low-quality silica fume, ultrafine mineral powder, fly ash microbeads and quartz sand, adding polycarboxylic acid water reducer and water, stirring to obtain slurry for about 5 minutes, adding steel fiber, and continuing stirring for 2 minutes to obtain ultra-high performance concrete.

[0076] Comparative Example 2

[0077] An ultra-high performance concrete comprises the following components by weight: 750 parts of cement, 90 parts of high-quality silica fume, 105 parts of ultra-fine mineral powder, 75 parts of fly ash microspheres, 900 parts of quartz sand, 163 parts of water, 11.3 parts of polycarboxylate water reducer, and steel fiber accounting for 3% of the volume of the ultra-high performance concrete; the water-cement ratio adopted is 0.16; wherein the ash content of the high-quality silica fume is 3.0%, the silicon dioxide content is 96.5%, the 28d compressive activity index thereof is 134%, and the water demand ratio is 115%;

[0078] The preparation method of the ultra-high performance concrete specifically comprises the following steps: after weighing cement, high-quality silica fume, ultra-fine mineral powder, fly ash microbeads and quartz sand, the weighed cement, high-quality silica fume, ultra-fine mineral powder, fly ash microbeads and quartz sand are evenly mixed, polycarboxylic acid water reducer and water are added, and slurry is obtained by stirring for about 5 minutes, steel fiber is added, and stirring is continued for 1 minute to obtain ultra-high performance concrete.

[0079] Comparative Example 3

[0080] An ultra-high performance concrete comprises the following components by weight: 750 parts of cement, 90 parts of low-quality silica fume, 105 parts of ultra-fine mineral powder, 75 parts of fly ash microspheres, 900 parts of AlN-silicon-alumina microporous aggregate, 204 parts of water, 11.3 parts of polycarboxylate water reducer, and steel fiber accounting for 3% of the volume of the ultra-high performance concrete; the water-binder ratio used is 0.2;

[0081] The specific preparation method of AlN-silica-alumina microporous aggregate and ultra-high performance concrete is the same as that of Example 2.

[0082] Comparative Example 4

[0083] An ultra-high performance concrete comprises the following components by weight: 750 parts of cement, 90 parts of low-quality silica fume, 105 parts of ultra-fine mineral powder, 75 parts of fly ash microspheres, 900 parts of quartz sand, 184 parts of water, 11.3 parts of polycarboxylate water reducer, and low-melting-point fiber-modified steel fiber accounting for 3% of the volume of the ultra-high performance concrete; the water-cement ratio used is 0.18;

[0084] The specific preparation methods of low melting point fiber modified steel fiber and ultra-high performance concrete are the same as those in Example 2.

[0085] The difference between this comparative example and Example 2 is that the specific preparation method of low hydration heat ultra-high performance large volume concrete is as follows: after the weighed cement, low-quality silica fume, ultrafine mineral powder, fly ash microbeads, and AlN-silica-alumina microporous aggregate are evenly mixed, polycarboxylic acid water reducer and water are added, and the slurry is stirred (the whole process takes about 7 minutes), low-melting point fiber modified steel fiber is added, and stirring is continued for 2 minutes to obtain low hydration heat ultra-high performance large volume concrete, and the rest is the same as Example 2.

[0086] The low hydration heat ultra-high performance mass concrete of Examples 1-7 of the present invention and the ultra-high performance concrete of Comparative Examples 1-5 were tested for adiabatic temperature rise, workability, mechanical properties, and shrinkage properties. The test results are shown in Tables 1 and Figure 1 shown.

[0087] As can be seen from Table 1, the ultra-high performance mass concrete with low hydration heat prepared by the method of the present invention has excellent mechanical properties, and its 28d compressive strength can reach 217MPa, and its 28d flexural strength can reach 37.6MPa, which is significantly better than the traditional ultra-high performance concrete prepared by conventional quartz sand and high-quality silica fume; the ultra-high performance mass concrete with low hydration heat obtained by the present invention has a lower adiabatic temperature rise, and its adiabatic temperature rise can be reduced by about 30°C compared with the existing conventional ultra-high performance concrete; the ultra-high performance mass concrete with low hydration heat prepared by the method of the present invention has excellent resistance to shrinkage cracking, and its 7d autogenous shrinkage can be as low as 210με, and its 180d shrinkage can be as low as 108με, which is significantly lower than the existing conventional ultra-high performance concrete.

[0088] Table 1 Performance test results of ultra-high performance concrete obtained from Examples 1 to 7 and Comparative Examples 1 to 2

[0089]

[0090] Figure 1 The hydration temperature rise test results of the ultra-high performance concrete obtained in Examples 2 and 3 and Comparative Example 2 show that the method of the present invention is used to prepare ultra-high performance large-volume concrete with low hydration heat, which can delay the hydration heat release process and reduce the adiabatic temperature rise.

[0091] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

[0092] The present invention is not limited to the above-mentioned embodiments. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention. The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.

Claims

1. A low hydration heat ultra-high performance mass concrete, characterized in that: The concrete comprises the following components by weight: 640-750 parts of cement, 90-110 parts of low-quality silica fume, 105-150 parts of ultrafine mineral powder, 75-106 parts of fly ash microspheres, 900 parts of AlN-silica-alumina microporous aggregate, 204-234 parts of water, 8.5-12.8 parts of polycarboxylic acid water reducer, and low-melting-point fiber-modified steel fiber accounting for 2-3% of the volume of the low-hydration heat ultra-high performance large-volume concrete; wherein the AlN-silica-alumina microporous aggregate is prepared from kaolin, low-quality silica fume, α-Al2O3 micropowder, and AlN-waste rubber powder as main raw materials, which are mixed with water, and then obtained by filter pressing, drying, calcining, crushing, and screening; The ash content of the low-quality silica ash is ≥4.5wt%, and the silicon dioxide content is <85wt%; the particle size of the ultrafine mineral powder is ≥325 mesh; the melting point of the low-melting-point fiber is 50-95°C; The mass ratio of the kaolin, low-quality silica fume, α-Al2O3 powder, and AlN-waste rubber powder-based powder is 1:(0.3-0.5):(0.08-0.1):(0.24-0.3); The AlN-waste rubber powder-based powder is obtained by placing a uniform mixture of waste rubber powder and α-Al2O3 powder in a nitrogen atmosphere for high-temperature reaction; wherein the α-Al2O3 powder accounts for 5-10% of the mass of the waste rubber powder; the high-temperature reaction adopts a temperature of 800-900°C and a time of 1-2h; The calcination temperature is 1200-1350° C., the time is 1-2 hours, and the heating rate is 5-10° C. / min.

2. The low hydration heat ultra-high performance mass concrete according to claim 1, characterized in that: In the step of adding water and mixing, water is added until the moisture content of the obtained mixture is 12-15%.

3. The low hydration heat ultra-high performance mass concrete according to claim 1, characterized in that: The calcination temperature is 1200-1350° C. and the calcination time is 1-2 hours.

4. The low hydration heat ultra-high performance mass concrete according to claim 1, characterized in that: The low-melting-point fiber-modified steel fiber is formed by spraying molten low-melting-point fiber onto the surface of the steel fiber; the diameter of the steel fiber is 0.18-0.22 mm, the length is 13-15 mm, and the aspect ratio is 60-70.

5. The ultra-high performance mass concrete with low hydration heat according to claim 1, characterized in that: The cement is ordinary Portland cement or Portland cement of grade 42.5 or above; the water demand ratio of fly ash microspheres is ≤95%, and the 28d compressive activity index is ≥110%.

6. The ultra-high performance mass concrete with low hydration heat according to claim 1, characterized in that: The water reduction rate of the polycarboxylate water reducer is ≥25%.

7. The method for preparing the low hydration heat ultra-high performance mass concrete according to any one of claims 1 to 6, characterized in that: The steps include: 1) Mix the weighed cement, low-quality silica fume, ultrafine mineral powder and fly ash microbeads evenly to obtain mixture A; 2) Take 20-30% of the mixture A, add water to it, stir evenly, add AlN-silicon-aluminum microporous aggregate, continue to stir evenly, and obtain the slurry-coated AlN-silicon-aluminum microporous aggregate mixture B; 3) Add the remaining mixture A and the polycarboxylate water-reducing agent to the obtained AlN-silicon-alumina microporous aggregate mixture B, stir evenly, and obtain a mixture C; 4) Add low-melting-point fiber-modified steel fiber to the obtained mixture C, and stir evenly to obtain the low-hydration heat ultra-high performance large-volume concrete.