A TOPCon solar cell and a method for preparing the same

During the preparation of TOPCon solar cells, the tunneling oxide layer was deposited by combining PECVD and PEALD, which solved the problems of poor uniformity of the tunneling oxide layer and the damage to the substrate surface, and improved the photoelectric conversion efficiency of the battery.

CN117174783BActive Publication Date: 2024-12-03JIANGSU MICROVIA NANO EQUIP TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202311334473.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-16
Publication Date
2024-12-03
Estimated Expiration
2043-10-16

AI Technical Summary

Technical Problem

The existing TOPCon solar cells have poor uniformity of tunneling oxide layers during the preparation process and cause damage to the substrate surface.

Method used

Using a combination of plasma enhanced chemical vapor deposition (PECVD) and plasma enhanced atomic deposition (PEALD), the first oxide layer is first deposited on the surface of the substrate, and then the second oxide layer is uniformly deposited on the basis of it, reducing plasma bombardment. Damage to the substrate surface and improve uniformity of the tunneled oxide layer.

Benefits of technology

The uniformity of the tunneled oxide layer is improved, the damage to the substrate surface by plasma bombardment is reduced, and the photoelectric conversion efficiency of TOPCon solar cells is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004495255730000091
    Figure BDA0004495255730000091
  • Figure BDA0004495255730000101
    Figure BDA0004495255730000101
  • Figure BDA0004495255730000111
    Figure BDA0004495255730000111
Patent Text Reader

Abstract

The present invention belongs to the technical field of solar cells, and specifically relates to a TOPCon solar cell and a preparation method thereof. The present invention combines the deposition of a tunneling oxide layer by using two methods of PECVD+PEALD. A thin oxide layer with a thickness of 0.1-0.5 nm is pre-deposited by PECVD. In the subsequent PEALD process, the thin oxide layer plays a role of chemical passivation on the surface of the substrate, and then a tunneling oxide layer is uniformly deposited on the basis of the oxide layer by using the PEALD process. The basic principle of this growth method is atomic layer deposition, and the oxide layer has good uniformity, and is less affected by the airflow, temperature, electric field, and radio frequency in the tube. It can avoid electroluminescence test failures such as stuck point printing caused by the tunneling oxide layer produced completely by laughing gas ionization, and reduce the damage effect of plasma bombardment on the substrate surface, which improves the conversion efficiency of the TOPCon solar cell to a certain extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solar cells, and in particular relates to a TOPCon solar cell and a preparation method thereof. Background Art

[0002] High-efficiency crystalline silicon solar cells - Tunnel Oxide Passivated Contact solar cells (TOPCon) are a new type of silicon solar cell proposed by the Fraunhofer Institute for Solar Energy in Germany in recent years. The cell uses a high-quality ultra-thin silicon oxide-doped polysilicon layer to achieve high-efficiency passivation of the entire back side of the cell and selective carrier collection.

[0003] In the field of crystalline silicon solar cell technology, tunneling oxide passivation contact (TOPCon) technology is an excellent cell passivation technology. In TOPCon cells, a passivation contact layer composed of a tunneling oxide layer and a polysilicon layer is deposited on the back of the cell, which can play a role in passivating the metal contact area on the back of the cell, reducing the recombination of photogenerated carriers in the metal contact area on the back of the cell, thereby improving cell performance.

[0004] In the prior art, plasma enhanced chemical vapor deposition (PECVD) technology is usually used to make the tunneling oxide layer on the back of the TOPCon battery. However, the direct use of nitrous oxide ionization to deposit the tunneling oxide layer has the following defects: the tunneling oxide layer continues to grow and thicken, and oxygen elements need to pass through the grown oxide layer to continue to react with silicon inside the substrate. Due to the influence of the airflow, temperature, electric field, and radio frequency in the tube during the deposition process, the tunneling oxide layer deposited by PECVD has poor uniformity; the bombardment of the substrate surface by plasma causes damage to the substrate surface.

[0005] In view of this, it is necessary to provide a method for preparing a TOPCon solar cell that can improve the uniformity of the tunneling oxide layer and avoid damage to the substrate surface. Summary of the invention

[0006] Therefore, the technical problem to be solved by the present invention is to overcome the defects of poor uniformity of the tunneling oxide layer and damage to the substrate surface in the preparation of TOPCon solar cells in the prior art, thereby providing a TOPCon solar cell and a preparation method thereof.

[0007] To this end, the present invention provides the following technical solutions:

[0008] The present invention provides a method for preparing a TOPCon solar cell, comprising a tunneling oxide layer, wherein the method for preparing the tunneling oxide layer comprises the following steps: depositing a first oxide layer on a substrate surface by plasma enhanced chemical vapor deposition, and depositing a second oxide layer by plasma enhanced atomic deposition, wherein the thickness of the first oxide layer is 0.1-0.5 nm.

[0009] In the present invention, there is no particular limitation on the composition of the tunnel oxide layer, and the material is usually silicon dioxide, but it can also be silicon oxynitride, but it is not mainstream.

[0010] Optionally, the first oxide layer has a thickness of 0.1-0.2 nm.

[0011] Optionally, the second oxide layer has a thickness of 0.3-2 nm.

[0012] Optionally, the method for preparing the TOPCon solar cell comprises the following steps:

[0013] S1, texturing, diffusion and alkali polishing of the substrate;

[0014] S2, depositing a tunnel oxide layer;

[0015] S3, depositing an intrinsic amorphous silicon layer;

[0016] S4, depositing a doped amorphous silicon layer;

[0017] S5, depositing a silicon dioxide layer;

[0018] S6, annealing, wet process, atomic layer deposition, coating, front and back electrode printing, sintering.

[0019] Among them, steps S2-S5 are all formed on the back side of the substrate; step S1 is to texture the entire substrate, diffuse on the front side, and alkali polishing generally only processes the back side. The specific operations of the steps of texture, diffusion, alkali polishing, wet method, atomic layer deposition, coating, front and back electrode printing, etc. in the present invention, and the operating parameters of steps S2-S5 are all conventional in the field and are not specifically limited here.

[0020] Optionally, in step S3, the intrinsic amorphous silicon layer is deposited by plasma enhanced chemical vapor deposition technology;

[0021] And / or, the thickness of the intrinsic amorphous silicon layer is 10-20 nm.

[0022] Optionally, in step S4, a doped amorphous silicon layer is deposited using a plasma enhanced chemical vapor deposition technique;

[0023] And / or, the thickness of the doped amorphous silicon layer is 20-130 nm;

[0024] And / or, the doped amorphous silicon layer is composed of a phosphorus-doped amorphous silicon layer.

[0025] Optionally, in step S5, a silicon dioxide layer is deposited using plasma enhanced chemical vapor deposition technology;

[0026] And / or, the thickness of the silicon dioxide layer is 10-15 nm.

[0027] Optionally, in step S1, the texturing step is to form a velvet shape on the surface of the substrate by alkali etching;

[0028] And / or, the diffusion step is performed by doping boron element on the front surface of the substrate;

[0029] And / or, the alkali polishing step is performed to form a polished surface on the back side of the substrate.

[0030] Optionally, in step S6, the operation of the wet process step is to remove the doped amorphous silicon layer at the edge of the substrate and remove the phosphosilicate glass layer on the back surface of the substrate;

[0031] And / or, the atomic layer deposition step is performed by depositing an aluminum oxide passivation layer on the front surface of the substrate;

[0032] And / or, the coating step is performed by coating a silicon nitride anti-reflection layer on the front and back sides of the substrate.

[0033] And / or, the sintering temperature is 650-850° C. and the sintering time is 1-2 min.

[0034] The present invention also provides a TOPCon solar cell prepared by the above preparation method.

[0035] The operating parameters in the preparation process of each functional layer in the present invention are conventional in the field. Typically, but not limiting, the operating parameters for depositing the first oxide layer may include: a laughing gas flow rate of 8000-10000sccm, a power of 8000-10000W, and a deposition time of 15-30s.

[0036] The operating parameters for depositing the second oxide layer may include: a total flow rate of argon gas carrying the silicon source of 2000-2500 sccm, a flow rate of nitrous oxide of 2000-2500 sccm, a deposition time of 1-2 min, and a power of 6000-9000W.

[0037] The intrinsic amorphous silicon layer film is deposited by introducing a mixed gas of argon and silane, the RF power is 8000-11000W, the deposition temperature is 400-450°C, the process pressure is 300-360pa, the deposition time is 4-8min, the argon flow rate is 6000-8000sccm, the silane flow rate is 2000-2500sccm, and the film thickness is controlled at 10-20nm.

[0038] Deposit the doped amorphous silicon layer thin film, introduce a mixed gas of argon, silane and phosphine, the RF power is 8000-10000W, the deposition temperature is 400-450℃, the process pressure is 300-360pa, the deposition time is 20-30min, the argon flow rate is 6000-8000sccm, the silane flow rate is 1500-2000sccm, the phosphine flow rate is 2500-3000sccm, and the film thickness is controlled at 20-130nm.

[0039] To deposit a silicon dioxide film, a mixed gas of silane and nitrous oxide is introduced, the RF power is 8000-10000 W, the deposition temperature is 400-450°C, the process pressure is 200-240 Pa, the deposition time is 1-2 min, the silane flow rate is 2500-3000 sccm, the nitrous oxide flow rate is 6000-8000 sccm, and the film thickness is controlled at 10-15 nm.

[0040] The technical solution of the present invention has the following advantages:

[0041] The preparation method of the TOPCon solar cell provided by the present invention changes the method of depositing the tunnel oxide layer completely by nitrous oxide ionization, and changes to a combination of plasma enhanced chemical vapor deposition (PECVD) + plasma enhanced atomic deposition (PEALD) to deposit the tunnel oxide layer. In the subsequent PEALD process, the grown first oxide layer plays a role of chemical passivation on the substrate surface, and then a second oxide layer is uniformly deposited on the basis of the oxide layer by the PEALD process. The basic principle of this growth method is atomic layer deposition, and the oxide layer has good uniformity, and is less affected by the airflow, temperature, electric field, and radio frequency in the tube. It can avoid the electroluminescence test (el) failure such as the stuck point print that occurs when the tunnel oxide layer is produced completely by nitrous oxide ionization, and reduce the damage effect of plasma bombardment on the substrate surface, thereby improving the conversion efficiency of the TOPCon solar cell to a certain extent. DETAILED DESCRIPTION

[0042] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0043] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0044] Example 1

[0045] This embodiment provides a method for preparing a TOPCon solar cell, which specifically includes the following steps:

[0046] Step 1: Perform conventional texturing, diffusion, and alkaline polishing treatments on the 182mm×182mm N-type substrate.

[0047] Step 2: The first oxide layer is deposited by nitrous oxide ionization on the alkali-polished substrate. The nitrous oxide flow rate for depositing the first oxide layer is 10000sccm, the power is 8000w, the deposition time is 15s, and the thickness is controlled at 0.1nm. On the basis of the first oxide layer, the second oxide layer is deposited by ion-enhanced atomic layer deposition, the total flow rate of argon carrying silicon source is 2000sccm, the nitrous oxide flow rate is 2400sccm, the deposition time is 90s, the power is 9000w, and the thickness is controlled at 1nm.

[0048] Step three, plasma enhanced chemical vapor deposition of intrinsic amorphous silicon film, introducing argon and silane mixed gas, RF power of 11000W, deposition temperature of 420℃, process pressure of 300pa, deposition time of 6min, argon flow rate of 6000sccm, silane flow rate of 2500sccm, film thickness controlled at 20nm.

[0049] Step 4: plasma enhanced chemical vapor deposition doped amorphous silicon film, introducing a mixed gas of argon, silane and phosphine, the RF power is 10000 W, the deposition temperature is 420°C, the process pressure is 300 Pa, the deposition time is 23 min, the argon flow rate is 6000 sccm, the silane flow rate is 2000 sccm, the phosphine flow rate is 3000 sccm, and the film thickness is controlled at 130 nm.

[0050] Step five, plasma enhanced chemical vapor deposition of silicon dioxide thin film, introducing silane and nitrous oxide mixed gas, the RF power is 10000 W, the deposition temperature is 420 ° C, the process pressure is 200 Pa, the deposition time is 1 min, the silane flow rate is 2500 sccm, the nitrous oxide flow rate is 6000 sccm, and the film thickness is controlled at 12 nm.

[0051] Step six, anneal the substrate after depositing Poly (doped amorphous silicon) at high temperature to activate the phosphorus atoms in the poly deposition. Then use RCA wet chemical cleaning to remove the doped amorphous silicon at the edge of the substrate and the phosphorus silicon glass on the surface. Then use atomic layer deposition to deposit the aluminum oxide film required on the front side (thickness is 1 to 3nm). Then coat the front and back sides with silicon nitride (front film 70-85nm, back film 80-100nm), and then go to the screen process for electrode printing and sintering (sintering temperature 650 to 850°C). Among them:

[0052] RCA wet: An industry standard wet cleaning process that uses hydrofluoric acid to remove the phosphosilicate glass layer on the substrate surface and alkali (potassium hydroxide) to remove the doped amorphous silicon layer at the edge of the substrate.

[0053] Atomic layer deposition: uses the chemical reaction of gaseous precursor molecules on the surface to deposit thin films layer by layer. During the deposition process, trimethylaluminum and water alternately enter the reaction chamber to generate aluminum oxide films. In this embodiment, the thickness of the aluminum film is controlled to be 2.5nm.

[0054] Front and back films: Plasma chemical vapor deposition is used to introduce ammonia and silane into the reaction chamber to deposit silicon nitride on the front and back of the substrate respectively. The thickness of the front film is controlled to be 80nm and the thickness of the back film is controlled to be 90nm.

[0055] Printing of front and back electrodes: Printing is carried out based on the basic principle that the slurry is passed through the mesh holes of the graphic part of the screen and the slurry is not passed through the mesh holes of the non-graphic part to prepare the front and back electrodes.

[0056] Sintering: The sintering temperature is 750°C. At high temperature, the silicon atoms in the substrate enter the molten metal electrode material to form an alloy system. After the temperature drops, the silicon atoms in the alloy system will recrystallize to form an epitaxial layer between the silicon wafer and the metal electrode, forming a good ohmic contact.

[0057] Example 2

[0058] This embodiment provides a method for preparing a TOPCon solar cell. Compared with Embodiment 1, the only difference is that step 2 is different, specifically, as follows:

[0059] The first oxide layer was deposited by nitrous oxide ionization on the substrate after alkaline polishing. The nitrous oxide flow rate for depositing the first oxide layer was 10000sccm, the power was 8000w, the deposition time was 15s, and the thickness was controlled at 0.1nm. On the basis of the first oxide layer, the second oxide layer was deposited by ion enhanced atomic layer deposition. The argon gas carrying silicon source flow rate was 2000sccm, the nitrous oxide flow rate was 2400sccm, the deposition time was 80s, the power was 9000W, and the thickness was controlled at 0.9nm.

[0060] Example 3

[0061] This embodiment provides a method for preparing a TOPCon solar cell. Compared with Embodiment 1, the only difference is that step 2 is different, specifically, as follows:

[0062] The first oxide layer was deposited by nitrous oxide ionization on the substrate after alkaline polishing. The nitrous oxide flow rate for depositing the first oxide layer was 10000sccm, the power was 8000w, the deposition time was 15s, and the thickness was controlled at 0.1nm. On the basis of the first oxide layer, the second oxide layer was deposited by ion enhanced atomic layer deposition. The argon gas carrying silicon source flow rate was 2000sccm, the nitrous oxide flow rate was 2400sccm, the deposition time was 70s, the power was 9000W, and the thickness was controlled at 0.8nm.

[0063] Example 4

[0064] This embodiment provides a method for preparing a TOPCon solar cell. Compared with Embodiment 1, the only difference is that step 2 is different, specifically, as follows:

[0065] The first oxide layer was deposited by plasma chemical vapor deposition on the alkali-polished substrate. The nitrous oxide flow rate was 10000sccm, the power was 8000w, the deposition time was 15s, and the thickness was controlled at 0.1nm. On the basis of the first oxide layer, the tunneling oxide layer was deposited by ion-enhanced atomic layer deposition. The total flow rate of argon gas carrying silicon source was 2000sccm, the nitrous oxide flow rate was 2400sccm, the deposition time was 100s, the power was 9000W, and the thickness was controlled at 1.2nm.

[0066] Comparative Example 1

[0067] This comparative example provides a method for preparing a TOPCon solar cell. Compared with Example 1, the only difference is that step 2 is different, specifically:

[0068] The alkali-polished substrate was subjected to plasma enhanced chemical vapor deposition tunneling oxide layer, with a nitrous oxide flow rate of 10000sccm, a power of 8000w, a deposition time of 120s, and a thickness controlled at 1nm.

[0069] Comparative Example 2

[0070] This comparative example provides a method for preparing a TOPCon solar cell. Compared with Example 1, the only difference is that step 2 is different, specifically:

[0071] The alkali-polished substrate was subjected to plasma enhanced chemical vapor deposition tunneling oxide layer, with a nitrous oxide flow rate of 10000sccm, a power of 8000w, a deposition time of 150s, and a thickness controlled at 1.1nm.

[0072] Comparative Example 3

[0073] This comparative example provides a method for preparing a TOPCon solar cell. Compared with Example 1, the only difference is that step 2 is different, specifically:

[0074] The tunneling oxide layer was deposited on the alkali-polished substrate. The argon gas carrying silicon source flow rate of the complete tunneling oxide layer PEALD was 2000sccm, the nitrous oxide flow rate was 2400sccm, the deposition time was 90s, the power was 9000W, and the thickness was controlled at 0.9nm.

[0075] Test Case

[0076] 1. Film uniformity test

[0077] The tunneling oxide layer was prepared according to the methods of each embodiment and comparative example of the present invention. During the film thickness test, when depositing the tunneling oxide layer (second oxide layer) of embodiment 1 / 2 / 3 / 4 and the complete tunneling oxide layer of comparative example 3, the deposition time was extended to 280 / 270 / 260 / 290s respectively, and the tunneling oxide layer of comparative example 1 / 2 was extended by 30min (since the thickness cannot be measured when it is too low, the actual film thickness is deposited to be about 4nm so that the thickness can be measured. As the running time increases, the thickness becomes thicker. If the thickness is uniform, it can also reflect the uniformity of growth by different methods). The film thickness test was compared. The differences between the example group and the comparative group are as follows: point 1 is the film thickness at the center of the substrate, and point 2-5 is the film thickness at the four corners of the substrate. The substrate was selected at the outer boat page and the middle boat page of the graphite boat. Since the PECVD furnace tube can usually process many sheets, A1-J15 are samples selected at different positions for testing. The specific results are shown in the table below:

[0078] Deposition time: The deposition time of the tunneling oxide layer (second oxide layer) deposited in Examples 1 / 2 / 3 / 4 and the complete tunneling oxide layer deposition time of Comparative Example 3 and the oxide layer thickness are in a linear relationship, and the thickness increases linearly with time. The deposition time and oxide layer thickness of Comparative Example 1 / 2 are in a nonlinear relationship, and the deposition rate gradually decreases with time, and it takes longer to deposit the same thickness.

[0079] Table 1

[0080]

[0081]

[0082]

[0083]

[0084] 2. Electrical performance test

[0085] The TOPCon solar cells obtained in each embodiment and comparative example were subjected to electrical performance tests, and the specific test steps and parameters were as follows:

[0086] Open circuit voltage: Use a voltmeter or a photoelectric conversion efficiency tester to measure the open circuit voltage of a solar cell when the solar cell is not connected to a load. At this time, the output current of the solar cell is zero.

[0087] Short-circuit current: Use an ammeter or a photoelectric conversion efficiency tester to measure the short-circuit current of a solar cell when the substrate is short-circuited. At this time, the output voltage of the solar cell is zero.

[0088] Conversion efficiency: Use a photoelectric conversion efficiency tester to measure the output power and absorbed light power of the solar cell under standard lighting conditions to calculate the conversion efficiency of the solar cell.

[0089] Fill factor: Use a photoelectric conversion efficiency tester to measure the output current and output voltage of the solar cell under standard lighting conditions to calculate the fill factor of the solar cell.

[0090] Series resistance: Use a resistance meter to measure the series resistance of a solar cell. Series resistance affects the output voltage and conversion efficiency of the solar cell.

[0091] Parallel resistance: Use a resistance meter to measure the parallel resistance of a solar cell. Parallel resistance affects the output current and conversion efficiency of the solar cell.

[0092] Leakage current: Use an ammeter or a photoelectric conversion efficiency tester to measure the leakage current of the solar cell when the solar cell load is not connected.

[0093] Table 2

[0094]

[0095] It can be seen from the data in Table 1 that the technical solution of the embodiment of the present invention increases the chemical passivation of the substrate surface, reduces the damage to the substrate surface caused by plasma bombardment, and improves the uniformity of the tunneling oxide layer (Table 1); at the same time, the photoelectric conversion efficiency of the TOPCon cell is improved without increasing the equipment (Table 2).

[0096] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A method for preparing a TOPCon solar cell, characterized in that: It includes a tunneling oxide layer arranged on the back side, and the preparation method of the tunneling oxide layer includes the following steps: depositing a first oxide layer on the surface of a substrate by plasma enhanced chemical vapor deposition, and depositing a second oxide layer on the basis of the first oxide layer by plasma enhanced atomic deposition, wherein the thickness of the first oxide layer is 0.1-0.5nm; the thickness of the second oxide layer is 0.3-2nm.

2. The method for preparing a TOPCon solar cell according to claim 1, characterized in that: The thickness of the first oxide layer is 0.1-0.2 nm.

3. The method for preparing a TOPCon solar cell according to any one of claims 1 to 2, characterized in that: The steps include: S1, texturing, diffusion and alkali polishing of the substrate; S2, depositing a tunnel oxide layer; S3, depositing an intrinsic amorphous silicon layer; S4, depositing a doped amorphous silicon layer; S5, depositing a silicon dioxide layer; S6, annealing, wet process, atomic layer deposition, coating, front and back electrode printing, sintering.

4. The method for preparing a TOPCon solar cell according to claim 3, characterized in that: In step S3, an intrinsic amorphous silicon layer is deposited using plasma enhanced chemical vapor deposition technology. 5 . The method for preparing a TOPCon solar cell according to claim 3 , wherein the thickness of the intrinsic amorphous silicon layer is 10-20 nm.

6. The method for preparing a TOPCon solar cell according to claim 3, characterized in that: In step S4, a doped amorphous silicon layer is deposited using plasma enhanced chemical vapor deposition technology; And / or, the thickness of the doped amorphous silicon layer is 20-130 nm; And / or, the doped amorphous silicon layer is composed of a phosphorus-doped amorphous silicon layer.

7. The method for preparing a TOPCon solar cell according to claim 3, characterized in that: In step S5, a silicon dioxide layer is deposited by plasma enhanced chemical vapor deposition technology; And / or, the thickness of the silicon dioxide layer is 10-15 nm.

8. The method for preparing a TOPCon solar cell according to claim 3, characterized in that: In step S1, the operation of the texturing step is to use alkali to etch the surface of the substrate into a velvet shape; And / or, the diffusion step is performed by doping boron element on the front surface of the substrate; And / or, the alkali polishing step is performed to form a polished surface on the back side of the substrate.

9. The method for preparing a TOPCon solar cell according to claim 3, characterized in that: In step S6, the operation of the wet process is to remove the doped amorphous silicon layer at the edge of the substrate and the phosphosilicate glass layer on the back surface of the substrate; And / or, the atomic layer deposition step is performed by depositing an aluminum oxide passivation layer on the front surface of the substrate; And / or, the coating step is performed by coating a silicon nitride anti-reflection layer on the front and back sides of the substrate; And / or, the sintering temperature is 750-800° C. and the sintering time is 1-2 min.

10. A TOPCon solar cell prepared according to the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Topcon solar cell and preparation method therefor

    EP4783782A1