A polyurethane coating with low radiation intensity and high mechanical strength, and its preparation method and application

The crosslinking agent prepared by reacting epoxy cyclohexane with isopropanolamine and isocyanate isophorone diisocyanate trimers in polyurethane coatings form a three-dimensional network structure, which solves the low radiation intensity in the prior art The problem of insufficient mechanical properties of polyurethane coatings achieves low radiation intensity, high mechanical strength and wear resistance, meeting flight safety needs.

CN117210118BActive Publication Date: 2024-11-12CHANGCHUN INSTITUTE OF APPLIED CHEMISTRY CHINESE ACADEMY OF SCIENCES
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202311312971.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-11
Publication Date
2024-11-12
Estimated Expiration
2043-10-11

AI Technical Summary

Technical Problem

The mechanical properties of existing low-radiation intensity polyurethane coatings are difficult to meet the requirements, and the radiation intensity of conventional coatings is high, which cannot meet the needs of flight safety. Especially in complex flight environments, the semiconductor film layer is susceptible to erosion and wear, affecting the radiation intensity.

Method used

The new crosslinking agent MIPA-CHO prepared by reacting epoxy cyclohexane with isopropanolamine combines the isocyanate isophorone diisocyanate trimer to form a three-dimensional network structure, which increases the tensile strength and modulus of the coating. , and obtain a low radiation intensity, high mechanical strength polyurethane coating through specific formulations and processes.

Benefits of technology

While ensuring low radiation intensity, the mechanical properties of the coating are significantly improved, the wear resistance and light transmittance are enhanced, the service life is extended, and the protection needs of aircraft canopy and other parts are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004488440050000041
    Figure BDA0004488440050000041
  • Figure BDA0004488440050000111
    Figure BDA0004488440050000111
  • Figure BDA0004488440050000112
    Figure BDA0004488440050000112
Patent Text Reader

Abstract

The present invention provides a polyurethane coating with low radiation intensity and high mechanical strength and a preparation method thereof, comprising the following raw materials in parts by weight: 16-20 parts of polyol, 0.5-2 parts of crosslinking agent, 6-8 parts of isocyanate, 0.1-0.2 parts of leveling agent, 0.05-0.2 parts of wetting agent, 0.2-0.4 parts of antioxidant, 0.3-0.4 parts of UV additive, 0.3-0.4 parts of light stabilizer, 0.1-0.15 parts of lubricant, 0.01-0.03 parts of catalyst, 70-75 parts of solvent; the crosslinking agent is obtained by reacting cyclohexene oxide with isopropanolamine. The polyurethane coating prepared in the present invention has low radiation intensity, and its other properties such as wear resistance, light transmittance, haze and mechanical strength are also at a high level within the test standard, and it is a comprehensive functional protective coating. The present invention also provides an application of the above-mentioned polyurethane coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic coatings, and in particular relates to a polyurethane coating with low radiation intensity and high mechanical strength, and a preparation method and application thereof. Background Art

[0002] The cockpit cover of a fighter jet is mainly made of polymethyl methacrylate (PMMA) or polycarbonate (PC). It has a high thermal radiation intensity in the atmospheric window band of 8 to 14 μm. With the continuous development of detection technology, it is very easy to be captured by detection equipment, affecting the safety of fighter jets. At present, the method of sputtering semiconductor film layers such as ITO on the surface of the cockpit cover is generally used to reduce the radiation intensity. However, due to the poor wear resistance of the cockpit cover substrate, in complex flight environments, such as deserts, Gobi and other sandy areas, the semiconductor film layer is very susceptible to erosion and wear, resulting in increased fog on the cockpit cover and increased radiation intensity, threatening flight safety. It needs to be coated on it for protection, but the conventional coating has high radiation intensity and cannot meet the use requirements.

[0003] Polyurethane elastomer is a block copolymer with a characteristic aminoester (-NH-COO-) group in the main chain of the molecule. It is composed of oligomer polyol as soft segment and polyisocyanate as hard segment connected alternately with chain extender through chemical reaction. The special microphase separation and soft and hard two-phase structure give polyurethane elastomer the excellent property of flexible modulus adjustment. After the 1950s, this material was used in cockpit covers, windshields and other parts of civil and military aircraft.

[0004] The mechanical properties of existing low-radiation intensity polyurethane coatings are difficult to meet the requirements, and the radiation intensity of film-forming materials that meet the requirements of physical and mechanical properties is relatively high. For example, in the schemes CN102732145A and CN114773975A, the method of adding fillers and changing the coating process is adopted to obtain a coating with a lower radiation rate, but this method is difficult to apply to optical-grade polyurethane coatings. Therefore, it is very necessary to develop a polyurethane transparent coating that maintains high mechanical strength while ensuring low radiation intensity. Summary of the invention

[0005] The purpose of the present invention is to provide a polyurethane coating with low radiation intensity and high mechanical strength, a preparation method and application thereof. The polyurethane coating of the present invention can effectively improve the mechanical properties of the coating while ensuring low radiation intensity (within the 8-14um band), while also having high light transmittance and strong adhesion.

[0006] The present invention provides a polyurethane coating with low radiation intensity and high mechanical strength, comprising the following raw materials in parts by weight:

[0007] 16-20 parts by weight of polyol, 0.5-2 parts by weight of crosslinking agent, 6-8 parts by weight of isocyanate, 0.1-0.2 parts by weight of leveling agent, 0.05-0.2 parts by weight of wetting agent, 0.2-0.4 parts by weight of antioxidant, 0.3-0.4 parts by weight of UV auxiliary agent, 0.3-0.4 parts by weight of light stabilizer, 0.1-0.15 parts by weight of lubricant, 0.01-0.03 parts by weight of catalyst, 70-75 parts by weight of solvent;

[0008] The cross-linking agent is obtained by reacting cyclohexene oxide with isopropanolamine.

[0009] Preferably, the weight proportion of the cyclohexene oxide is 70 to 75 parts, and the weight proportion of the isopropanolamine is 25 to 30 parts.

[0010] Preferably, the temperature for the reaction of cyclohexene oxide and isopropanolamine is 135-150° C., and the reaction time is 6-8 hours.

[0011] Preferably, the polyol is a polyolefin polyol; the molecular weight of the polyol is 1000 to 3000 g / mol.

[0012] Preferably, the isocyanate is one or more of 4,4'-dicyclohexylmethane diisocyanate, hexamethylene diisocyanate trimer, and isophorone diisocyanate trimer.

[0013] Preferably, the leveling agent is one or more of a short-chain fluorocarbon modified polymer leveling agent, a short-chain fluorocarbon modified polyacrylate leveling agent and a modified silane leveling agent;

[0014] The wetting agent is a polyether modified siloxane wetting agent;

[0015] The light stabilizer is light stabilizer 770;

[0016] The antioxidant is one or more of antioxidant 264, antioxidant 168 and antioxidant 1010;

[0017] The ultraviolet additive is ultraviolet additive 531;

[0018] The lubricant is a silicone lubricant;

[0019] The catalyst is dibutyltin dilaurate;

[0020] The solvent is one or more of cyclohexanone, dioxane and xylene.

[0021] The present invention provides a method for preparing a polyurethane coating with low radiation intensity and high mechanical strength as described above, comprising the following steps:

[0022] A) dehydrating the polyol under vacuum conditions;

[0023] B) stirring and mixing the dehydrated polyol, crosslinking agent, isocyanate, leveling agent, wetting agent, light stabilizer, antioxidant, UV additive, slip agent, catalyst and solvent to obtain a polyurethane coating;

[0024] C) The polyurethane coating is applied and then cured to obtain a polyurethane coating with low radiation intensity and high mechanical strength.

[0025] Preferably, the temperature of vacuum dehydration in step A) is 100-140° C., and the time of vacuum dehydration is 1-3 hours.

[0026] Preferably, the curing temperature in step C) is 50-70° C. and the curing time is 6-10 hours.

[0027] The present invention provides the use of the polyurethane coating with low radiation intensity and high mechanical strength as described above in aircraft protective coating.

[0028] The present invention provides a polyurethane coating with low radiation intensity and high mechanical strength, comprising the following raw materials in parts by weight: 16 to 20 parts by weight of polyol, 0.5 to 2 parts by weight of crosslinking agent, 6 to 8 parts by weight of isocyanate, 0.1 to 0.2 parts by weight of leveling agent, 0.05 to 0.2 parts by weight of wetting agent, 0.2 to 0.4 parts by weight of antioxidant, 0.3 to 0.4 parts by weight of UV additive, 0.3 to 0.4 parts by weight of light stabilizer, 0.1 to 0.15 parts by weight of lubricant, 0.01 to 0.03 parts by weight of catalyst, and 70 to 75 parts by weight of solvent; the crosslinking agent is obtained by the reaction of cyclohexene oxide and isopropanolamine. The present invention develops a new crosslinking agent MIPA-CHO, the epoxy group in cyclohexene oxide reacts with the amino group in isopropanolamine through ring-opening reaction, and the synthesized crosslinking agent has three secondary hydroxyl groups, which react with -NCO to form a three-dimensional network structure. More rigid ring structures are introduced into the polyurethane molecular chain through CHO, which improves the tensile strength and modulus of the coating. At the same time, the use of trifunctional isocyanate isophorone diisocyanate trimer increases the crosslinking density and increases the molecular cohesive energy. Under the dual action of the two, the mechanical properties of the coating are effectively improved. In addition, since the density of high-radiation groups such as carbamate remains stable, while improving the mechanical properties of the coating, low radiation intensity is guaranteed, thereby extending the service life of the functional polyurethane coating. Experimental data show that the polyurethane coating prepared in the present invention has low radiation intensity, while its other properties such as wear resistance, light transmittance, haze and mechanical strength are also at a higher level within the test standard, and it is a functional protective coating with strong comprehensiveness. DETAILED DESCRIPTION

[0029] The present invention provides a polyurethane coating with low radiation intensity and high mechanical strength, comprising the following raw materials in parts by weight:

[0030] 16-20 parts by weight of polyol, 0.5-2 parts by weight of crosslinking agent, 6-8 parts by weight of isocyanate, 0.1-0.2 parts by weight of leveling agent, 0.05-0.2 parts by weight of wetting agent, 0.2-0.4 parts by weight of antioxidant, 0.3-0.4 parts by weight of UV auxiliary agent, 0.3-0.4 parts by weight of light stabilizer, 0.1-0.15 parts by weight of lubricant, 0.01-0.03 parts by weight of catalyst, 70-75 parts by weight of solvent;

[0031] The cross-linking agent is obtained by reacting cyclohexene oxide with isopropanolamine.

[0032] In the present invention, the polyol is preferably a polyolefin polyol, more preferably a combination of polyolefin polyols of different molecular weights, the molecular weight range of the polyol is preferably 1000-3000 g / mol, specifically, in an embodiment of the present invention, a polybutadiene polyol with a molecular weight of 3000 g / mol and a polybutadiene polyol with a molecular weight of 1000 / mol can be used, specifically, in an embodiment of the present invention, the mass ratio of the polybutadiene polyol with a molecular weight of 3000 g / mol and the polybutadiene polyol with a molecular weight of 1000 / mol is preferably (4-5):1.

[0033] The weight fraction of the polyol is preferably 16 to 20 parts, such as 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, preferably a range value with any of the above values ​​as the upper or lower limit.

[0034] In the present invention, the weight proportion of the cross-linking agent is preferably 0.5 to 2 parts, more preferably 1 to 1.5 parts, such as 0.5 parts, 1 parts, 1.5 parts, 2 parts, preferably a range value with the above arbitrary numerical values ​​as the upper or lower limit; the cross-linking agent is preferably a compound obtained by reacting cyclohexene oxide and isopropanolamine, as shown in Formula I. In the present invention, based on the total weight of cyclohexene oxide and isopropanolamine as 100 parts, the weight proportion of the cyclohexene oxide is preferably 70 to 75 parts, such as 70 parts, 71 parts, 72 parts, 73 parts, 74 parts, 75 parts, preferably a range value with the above arbitrary numerical values ​​as the upper or lower limit, the weight proportion of the isopropanolamine is preferably 25 to 30 parts, such as 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, preferably a range value with the above arbitrary numerical values ​​as the upper or lower limit.

[0035]

[0036] In the present invention, the temperature of the reaction of cyclohexene oxide and isopropanolamine is preferably 135-150°C, more preferably 140-145°C, such as 135°C, 136°C, 137°C, 138°C, 139°C, 140°C, 141°C, 142°C, 143°C, 144°C, 145°C, 146°C, 147°C, 148°C, 149°C, 150°C, preferably with any of the above values ​​as the upper or lower limit of the range value; the reaction time is preferably 6-8 hours, more preferably 7-8 hours.

[0037] In the present invention, the weight proportion of the crosslinking agent is preferably 1 to 2 parts, such as 1 part, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts, 2 parts, preferably a range value with any of the above values ​​as the upper or lower limit.

[0038] In the present invention, the isocyanate is one or more of 4,4'-dicyclohexylmethane diisocyanate, hexamethylene diisocyanate trimer, and isophorone diisocyanate trimer; the weight proportion of the isocyanate is preferably 6 to 8 parts, such as 6 parts, 7 parts, and 8 parts, preferably a range value with any of the above values ​​as the upper or lower limit.

[0039] The present invention preferably uses isophorone diisocyanate trimer to increase the crosslinking density. The combination of 4,4'-dicyclohexylmethane diisocyanate and isophorone diisocyanate trimer can simultaneously improve the strength and toughness of the coating. The reaction rate of hexamethylene diisocyanate trimer in the process of the present invention is too fast, so it is preferably used in a small amount or used in combination with isophorone diisocyanate trimer.

[0040] The leveling agent is preferably one or more of a short-chain fluorocarbon modified polymer leveling agent, a short-chain fluorocarbon modified polyacrylate leveling agent and a modified silane leveling agent; the weight proportion of the leveling agent is preferably 0.1 to 0.2 parts, such as 0.1 parts, 0.11 parts, 0.12 parts, 0.13 parts, 0.14 parts, 0.15 parts, 0.16 parts, 0.17 parts, 0.18 parts, 0.19 parts, 0.2 parts, preferably a range value with any of the above values ​​as the upper or lower limit.

[0041] The wetting agent is a polyether modified silicone wetting agent; the weight proportion of the wetting agent is preferably 0.05 to 0.2 parts, such as 0.05 parts, 0.06 parts, 0.07 parts, 0.08 parts, 0.09 parts, 0.1 parts, 0.11 parts, 0.12 parts, 0.13 parts, 0.14 parts, 0.15 parts, 0.16 parts, 0.17 parts, 0.18 parts, 0.19 parts, 0.2 parts, preferably a range value with any of the above values ​​as the upper or lower limit.

[0042] The light stabilizer is preferably light stabilizer 770, and the weight amount of the light stabilizer is preferably 0.3 to 0.4 parts.

[0043] The antioxidant is one or more of antioxidant 264, antioxidant 168 and antioxidant 1010; the weight proportion of the antioxidant is preferably 0.2 to 0.4 parts, such as 0.2 parts, 0.3 parts, 0.4 parts, preferably a range value with any of the above values ​​as the upper or lower limit.

[0044] The ultraviolet auxiliary agent is preferably ultraviolet auxiliary agent 531; the weight proportion of the ultraviolet auxiliary agent is preferably 0.3 to 0.4 parts.

[0045] The lubricant is a silicone lubricant; the lubricant is preferably 0.1 to 0.15 parts, such as 0.1 parts, 0.11 parts, 0.12 parts, 0.13 parts, 0.14 parts, 0.15 parts, preferably a range value with any of the above values ​​as the upper or lower limit.

[0046] The catalyst is dibutyltin dilaurate; the weight proportion of the catalyst is preferably 0.01 to 0.03 parts, such as 0.01 parts, 0.02 parts, 0.03 parts, preferably a range value with any of the above values ​​as the upper or lower limit.

[0047] The solvent is one or more of cyclohexanone, dioxane and xylene; the weight proportion of the solvent is preferably 70 to 75 parts, such as 70 parts, 71 parts, 72 parts, 73 parts, 74 parts, 75 parts, preferably a range value with any of the above values ​​as the upper or lower limit.

[0048] The present invention also provides a method for preparing the polyurethane coating with low radiation intensity and high mechanical strength as claimed in claim 1, comprising the following steps:

[0049] A) dehydrating the polyol under vacuum conditions;

[0050] B) stirring and mixing the dehydrated polyol, crosslinking agent, isocyanate, leveling agent, wetting agent, light stabilizer, antioxidant, UV additive, slip agent, catalyst and solvent to obtain a polyurethane coating;

[0051] C) The polyurethane coating is applied and then cured to obtain a polyurethane coating with low radiation intensity and high mechanical strength.

[0052] In the present invention, the types and amounts of the polyols, crosslinking agents, isocyanates, leveling agents, wetting agents, light stabilizers, antioxidants, lubricants, catalysts and solvents are consistent with the types and amounts of the polyols, crosslinking agents, isocyanates, leveling agents, wetting agents, light stabilizers, antioxidants, lubricants, catalysts and solvents described above, and the present invention will not be repeated here.

[0053] In the present invention, the temperature of vacuum dehydration is preferably 100-140°C, more preferably 110-130°C, such as 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, preferably a range value with any of the above values ​​as the upper or lower limit; the time of vacuum dehydration is preferably 1-3 hours, more preferably 2-3 hours.

[0054] In the present invention, all materials are preferably stirred at 25° C. for 2 to 3 hours and allowed to stand for 3 to 4 hours to eliminate bubbles to obtain a polyurethane coating.

[0055] The polyurethane coating is coated on the surface of a substrate, and then cured after being surface dried at room temperature to obtain a polyurethane coating with low radiation intensity and high mechanical strength.

[0056] In the present invention, the substrate is preferably an ITO-PMMA substrate; the curing temperature is preferably 50 to 70° C., more preferably 55 to 60° C.; the curing time is preferably 6 to 10 hours, more preferably 7 to 8 hours.

[0057] The low radiation intensity and high mechanical strength polyurethane coating described in the present invention is used for polymethyl methacrylate (PMMA) material sputtered with an ITO semiconductor film layer or polycarbonate (PC) material sputtered with an ITO semiconductor film layer, especially for coating protection of products such as aircraft canopies that require reduced radiation intensity.

[0058] The present invention provides a polyurethane coating with low radiation intensity and high mechanical strength, comprising the following raw materials in parts by weight: 16 to 20 parts by weight of polyol, 0.5 to 2 parts by weight of crosslinking agent, 6 to 8 parts by weight of isocyanate, 0.1 to 0.2 parts by weight of leveling agent, 0.05 to 0.2 parts by weight of wetting agent, 0.2 to 0.4 parts by weight of antioxidant, 0.3 to 0.4 parts by weight of UV additive, 0.3 to 0.4 parts by weight of light stabilizer, 0.1 to 0.15 parts by weight of lubricant, 0.01 to 0.03 parts by weight of catalyst, and 70 to 75 parts by weight of solvent; the crosslinking agent is obtained by the reaction of cyclohexene oxide and isopropanolamine. The present invention develops a new crosslinking agent MIPA-CHO, the epoxy group in cyclohexene oxide reacts with the amino group in isopropanolamine through ring-opening reaction, and the synthesized crosslinking agent has three secondary hydroxyl functional groups, which react with -NCO to form a three-dimensional network structure. More rigid ring structures are introduced into the polyurethane molecular chain through CHO, which improves the tensile strength and modulus of the coating. At the same time, the use of trifunctional isocyanate isophorone diisocyanate trimer increases the crosslinking density and increases the molecular cohesive energy. Under the dual action of the two, the mechanical properties of the coating are effectively improved. In addition, since the density of high-radiation groups such as carbamate remains stable, while improving the mechanical properties of the coating, low radiation intensity is guaranteed, thereby extending the service life of the functional polyurethane coating. Experimental data show that the polyurethane coating prepared in the present invention has low radiation intensity, while its other properties such as wear resistance, light transmittance, haze and mechanical strength are also at a higher level within the test standard, and it is a functional protective coating with strong comprehensiveness.

[0059] In order to further illustrate the present invention, a polyurethane coating with low radiation intensity and high mechanical strength, a preparation method and application thereof provided by the present invention are described in detail below in combination with embodiments, but it should not be construed as limiting the scope of protection of the present invention.

[0060] Example 1: Combination of polyol, crosslinker and isophorone diisocyanate trimer

[0061] A transparent polyurethane coating with low radiation and high mechanical properties, the specific preparation method is as follows:

[0062] Add polybutadiene polyol (molecular weight 3000g / mol, molecular weight 1000g / mol) into the reactor and remove water at 120℃ under vacuum for 2h. Take 14.6 parts of the above dehydrated polybutadiene polyol (molecular weight 3000g / mol) and 3.2 parts of polybutadiene polyol (molecular weight 1000g / mol) into the reactor and add MIPA-CHO 1.3 parts, 41 parts of cyclohexanone, 16 parts of dioxane, 16 parts of xylene, 6.4 parts of isophorone diisocyanate trimer, 0.015 parts of dibutyltin dilaurate, 0.15 parts of short-chain fluorocarbon modified polymer leveling agent, 0.13 parts of polyether modified siloxane wetting agent, 0.3 parts of 531 ultraviolet absorber, 0.3 parts of 770 light stabilizer, 0.2 parts of 264 antioxidant, 0.2 parts of 168 antioxidant, 0.11 parts of silicone lubricant, stir at 25°C for 2h, let stand for 3h to eliminate bubbles, and obtain a low-radiation intensity transparent polyurethane coating. The coating is applied to the surface of an ITO-PMMA substrate, and after surface drying at room temperature, it is cured at 60°C for 8h to obtain a low-radiation transparent polyurethane coating with a hard segment content of 30.2%.

[0063] Example 2: Combination of polyol, crosslinker and three isocyanates

[0064] A transparent polyurethane coating with low radiation and high mechanical properties, the specific preparation method is as follows:

[0065] Add polybutadiene polyol (molecular weight 3000g / mol, molecular weight 1000g / mol) into the reactor and remove water at 120℃ under vacuum for 2h. Take 14.6 parts of the above dehydrated polybutadiene polyol (molecular weight 3000g / mol) and 3.2 parts of polybutadiene polyol (molecular weight 1000g / mol) into the reactor and add MIPA-CHO 1.3 parts, 41 parts of cyclohexanone, 16 parts of dioxane, 16 parts of xylene, 4.7 parts of isophorone diisocyanate trimer, 0.9 parts of 4,4'-dicyclohexylmethane diisocyanate, 0.7 parts of hexamethylene diisocyanate trimer, 0.015 parts of dibutyltin dilaurate, 0.15 parts of short-chain fluorocarbon modified polymer leveling agent, 0.13 parts of polyether modified siloxane wetting agent, 0.3 parts of 531 ultraviolet absorber, 0.3 parts of 770 light stabilizer, 0.2 parts of 264 antioxidant, 0.2 parts of 168 antioxidant, 0.11 parts of silicone lubricant, stir at 25°C for 2h, let stand for 3h to eliminate bubbles, and obtain a low-radiation intensity transparent polyurethane coating. The coating is applied to the surface of the ITO-PMMA substrate, and after surface drying at room temperature, it is cured at 60°C for 8h to obtain a low-radiation transparent polyurethane coating with a hard segment content of 29.5%.

[0066] Example 3: Combination of polyol, crosslinker and two isocyanates

[0067] A transparent polyurethane coating with low radiation and high mechanical properties, the specific preparation method is as follows:

[0068] Add polybutadiene polyol (molecular weight 3000g / mol, molecular weight 1000g / mol) into the reactor and remove water at 120℃ under vacuum for 2h. Take 14.6 parts of the above dehydrated polybutadiene polyol (molecular weight 3000g / mol) and 3.2 parts of polybutadiene polyol (molecular weight 1000g / mol) into the reactor and add MIPA-CHO 1.3 parts, cyclohexanone 41 parts, dioxane 16 parts, xylene 16 parts, isophorone diisocyanate trimer 5.1 parts, hexamethylene diisocyanate trimer 1.3 parts, dibutyltin dilaurate 0.015 parts, short-chain fluorocarbon modified polymer leveling agent 0.15 parts, polyether modified siloxane wetting agent 0.13 parts, 531 ultraviolet absorber 0.3 parts, 770 light stabilizer 0.3 parts, 264 antioxidant 0.2 parts, 168 antioxidant 0.2 parts, silicone slip agent 0.12 parts, temperature controlled stirring at 25 ° C for 2h, standing for 3h to eliminate bubbles, to obtain a low-radiation intensity transparent polyurethane coating, the coating is applied to the surface of the ITO-PMMA substrate, and after surface drying at room temperature, it is cured at 60 ° C for 8h to obtain a low-radiation transparent polyurethane coating with a hard segment content of 30.2%.

[0069] Comparative Example 1

[0070] This comparative example provides a low-radiation transparent polyurethane coating and a preparation method thereof. The difference between this comparative example and Example 1 is that Example 1 uses the developed crosslinking agent MIPA-CHO to prepare the coating, while this comparative example uses chain extenders N,N"-di-tert-butylethylenediamine and trimethylolpropane.

[0071] Add polybutadiene polyol (molecular weight 3000g / mol, molecular weight 1000g / mol) into the reactor and remove water under vacuum at 120℃ for 2h. Take 14.6 parts of the above dehydrated polybutadiene polyol (molecular weight 3000g / mol) and 3.2 parts of polybutadiene polyol (molecular weight 1000g / mol) into the reactor, add 0.8 parts of N,N"-di-tert-butylethylenediamine, 0.32 parts of trimethylolpropane, 41 parts of cyclohexanone, 16 parts of dioxane, 16 parts of xylene, 4.7 parts of isophorone diisocyanate trimer, 0.9 parts of 4,4'-dicyclohexylmethane diisocyanate, 0.7 parts of hexamethylene diisocyanate trimer, 0.015 parts of dibutyltin dilaurate, and short-chain fluorocarbon modified 0.15 parts of polymer leveling agent, 0.13 parts of polyether modified siloxane wetting agent, 0.3 parts of 531 ultraviolet absorber, 0.3 parts of 770 light stabilizer, 0.2 parts of 264 antioxidant, 0.2 parts of 168 antioxidant, 0.22 parts of perfluorobutanol, 0.12 parts of silicone lubricant, stirred at 25°C for 2 hours, let stand for 3 hours to eliminate bubbles, and obtain a low-radiation intensity transparent polyurethane coating. The coating was applied to the surface of ITO-PMMA substrate, dried at room temperature, and then cured at 60°C for 8 hours to obtain a low-radiation transparent polyurethane coating with a hard segment content of 29.4%.

[0072] Comparative Example 2

[0073] Add polybutadiene polyol (molecular weight 3000g / mol, molecular weight 1000g / mol) into the reactor and remove water at 120℃ under vacuum for 2h. Take 14.6 parts of the above dehydrated polybutadiene polyol (molecular weight 3000g / mol) and 3.2 parts of polybutadiene polyol (molecular weight 1000g / mol) into the reactor, add 0.8 parts of trimethylolpropane, 41 parts of cyclohexanone, 16 parts of dioxane, 16 parts of xylene, 6.4 parts of isophorone diisocyanate trimer, 0.015 parts of dibutyltin dilaurate, 0.15 parts of short-chain fluorocarbon modified polymer leveling agent, and 0.13 parts of polyether modified siloxane wetting agent. The mixture was stirred at 25°C for 2 h, allowed to stand for 3 h to eliminate bubbles, and a low-radiation intensity transparent polyurethane coating was obtained. The coating was applied to the surface of the ITO-PMMA substrate, and after being dried at room temperature, it was cured at 60°C for 8 h to obtain a low-radiation transparent polyurethane coating with a hard segment content of 28.8%.

[0074] Comparative Example 3

[0075] Add polybutadiene polyol (molecular weight 3000g / mol, molecular weight 1000g / mol) into the reactor and remove water under vacuum at 120℃ for 2h. Take 14.6 parts of the above dehydrated polybutadiene polyol (molecular weight 3000g / mol) and 3.2 parts of polybutadiene polyol (molecular weight 1000g / mol) into the reactor, add 1.25 parts of N,N"-di-tert-butylethylenediamine, 41 parts of cyclohexanone, 16 parts of dioxane, 16 parts of xylene, 6.4 parts of isophorone diisocyanate trimer, 0.015 parts of dibutyltin dilaurate, 0.15 parts of short-chain fluorocarbon modified polymer leveling agent, and 0.015 parts of polyether modified siloxane wetting agent. .13 parts, 531 ultraviolet absorber 0.3 parts, 770 light stabilizer 0.3 parts, 264 antioxidant 0.2 parts, 168 antioxidant 0.22 parts of perfluorobutanol, 0.12 parts of silicone lubricant, stirred at 25°C for 2 hours, let stand for 3 hours to eliminate bubbles, and obtain a low-radiation intensity transparent polyurethane coating, which is applied to the surface of ITO-PMMA substrate, dried at room temperature and then cured at 60°C for 8 hours to obtain a low-radiation transparent polyurethane coating with a hard segment content of 30.1%.

[0076] Performance Testing

[0077] The low-emissivity transparent polyurethane coatings obtained in Examples 1-3 were tested as follows:

[0078] Light transmittance and haze test: in accordance with GB / T 2410-2008 "Determination of light transmittance and haze of transparent plastics".

[0079] Wear resistance: According to ASTM F735-11, the reciprocating sand oscillation abrasion tester (Taber6160) was used for testing, and 100 strokes were performed at a cycle speed of 150 strokes / minute. The degree of wear was measured by the change in the transmittance and haze of the coating before and after the test, which is expressed as Δ transmittance / Δ haze in the table below.

[0080] Mechanical properties: According to the standard test method of GB 13022-1991, the tensile strength, elongation and modulus of the coating were measured.

[0081] Radiation intensity: The radiation intensity of the coating was tested using Bruker's INVENIO R and A540 instruments, using the blackbody comparison method.

[0082] Durability: Field tests were conducted in accordance with GB / 9276-1966. The direction was 45° south, the total test duration was 30 days, the test time was June-July, and the test area was Changchun. Changchun is located at 43° north latitude and 125° east longitude. The climate is in the transition zone between the humid eastern mountainous area and the semi-arid western plain area, and belongs to the temperate continental semi-humid monsoon climate type.

[0083] The radiation intensities of the test samples of Example 1, Example 2, Example 3 and Comparative Example 1 were 462.29, 459.61, 465.05 and 454.71 W / (m 2 ·K 4 ). Compared with the radiation intensity of ordinary protective coatings, it is mostly 628.67-663.60W / (m 2 ·K 4 ) significantly decreased.

[0084] The coating test results before field irradiation are shown in Table 1:

[0085] Table 1 Test results of coating before external field irradiation in the embodiment of the present invention

[0086]

[0087] It can be seen from the contents of Table 1 that the anti-dust and wear-resistant coatings prepared in Examples 1-3 have an adhesion grade of 5B, a transmittance greater than 92%, and a haze lower than 0.5. After the Taber 100 stroke friction test, the increase in the transmittance of the coating is within 0.5%, and the increase in the haze is less than 0.1. Among them, the tensile strength of the coating obtained in Example 1 is 19.37 MPa, and the modulus is 23.34 MPa. Compared with the coating obtained in Comparative Example 1, the mechanical properties are significantly improved.

[0088] The test results after field irradiation are shown in Table 2:

[0089] Table 2 Test results of coating after external field irradiation in the embodiment of the present invention

[0090]

[0091]

[0092] It can be seen from the contents of Table 2 that after one month of external field irradiation, various indicators of the coatings of the comparative example and embodiments 1-3 have decreased.

[0093] Compared with Example 1, the transmittance of the low-emissivity coating obtained in Comparative Example 1 decreased to 91.1%, and the haze increased to 2.08. After the Taber 100 stroke friction test, the transmittance and haze increased by 0.91% and 1.47, and the optical properties and wear resistance of the coating were significantly deteriorated.

[0094] Compared with Example 1, the tensile strength of the low-radiative coating obtained in Comparative Example 1 was reduced to 7.25 MPa and the modulus was reduced to 4.16 MPa after external field irradiation, and the mechanical properties of the coating were significantly reduced.

[0095] In summary, compared with Examples 1-3, the coating of Comparative Example 1 has significantly reduced performance indicators, especially mechanical properties, after field irradiation, and poor durability. However, after 30 days of field testing, the polyurethane transparent coating prepared in the present invention has other properties such as wear resistance, light transmittance and haze that can maintain a high level within the test standard, while ensuring relatively excellent mechanical properties, and extending the protective performance and service life of the functional transparent polyurethane coating.

[0096] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A polyurethane coating with low radiation intensity and high mechanical strength, comprising the following raw materials in parts by weight: 16-20 parts by weight of polyol, 0.5-2 parts by weight of crosslinking agent, 6-8 parts by weight of isocyanate, 0.1-0.2 parts by weight of leveling agent, 0.05-0.2 parts by weight of wetting agent, 0.2-0.4 parts by weight of antioxidant, 0.3-0.4 parts by weight of UV auxiliary agent, 0.3-0.4 parts by weight of light stabilizer, 0.1-0.15 parts by weight of lubricant, 0.01-0.03 parts by weight of catalyst, 70-75 parts by weight of solvent; The cross-linking agent is obtained by reacting cyclohexene oxide and isopropanolamine, wherein the weight proportion of the cyclohexene oxide is 70 to 75 parts, and the weight proportion of the isopropanolamine is 25 to 30 parts; The isocyanate is one or more of 4,4'-dicyclohexylmethane diisocyanate, hexamethylene diisocyanate trimer, and isophorone diisocyanate trimer. The isocyanate at least contains hexamethylene diisocyanate trimer or isophorone diisocyanate trimer.

2. The polyurethane coating according to claim 1, It is characterized in that The temperature for the reaction of cyclohexene oxide and isopropanolamine is 135-150° C., and the reaction time is 6-8 hours.

3. The polyurethane coating according to claim 1, It is characterized in that The polyol is a polyolefin polyol; the molecular weight of the polyol is 1000-3000 g / mol.

4. The polyurethane coating according to claim 1, It is characterized in that The leveling agent is one or more of a short-chain fluorocarbon modified polymer leveling agent, a short-chain fluorocarbon modified polyacrylate leveling agent and a modified silane leveling agent; The wetting agent is a polyether modified siloxane wetting agent; The light stabilizer is light stabilizer 770; The antioxidant is one or more of antioxidant 264, antioxidant 168 and antioxidant 1010; The ultraviolet additive is ultraviolet additive 531; The lubricant is a silicone lubricant; The catalyst is dibutyltin dilaurate; The solvent is one or more of cyclohexanone, dioxane and xylene.

5. The method for preparing the polyurethane coating with low radiation intensity and high mechanical strength as claimed in claim 1, The following steps are involved: A) dehydrating the polyol under vacuum conditions; B) stirring and mixing the dehydrated polyol, crosslinking agent, isocyanate, leveling agent, wetting agent, light stabilizer, antioxidant, UV additive, slip agent, catalyst and solvent to obtain a polyurethane coating; C) The polyurethane coating is applied and then cured to obtain a polyurethane coating with low radiation intensity and high mechanical strength.

6. The preparation method according to claim 5, It is characterized in that The temperature of vacuum dehydration in step A) is 100-140° C.; the time of vacuum dehydration is 1-3 hours.

7. The preparation method according to claim 5, It is characterized in that The curing temperature in step C) is 50-70° C. and the curing time is 6-10 hours.

8. Use of the polyurethane coating with low radiation intensity and high mechanical strength as claimed in any one of claims 1 to 4 in aircraft protective coating.

Citation Information

Patent Citations

  • Bi-component polyurethane coating with low infrared emissivity and preparation method thereof

    CN102732145A

  • Water-based infrared camouflage coating as well as preparation method and application thereof

    CN114773975A

  • Polyurethane coating compositions

    CN107636096A

  • Adhesive sheet for semiconductor processing

    CN109312199A

  • Polyurethane composition

    CN1608089A