Alkali-free self-thickening gradient core-shell acrylic emulsion and preparation method thereof
By designing an acrylic emulsion with a gradient core-shell structure with alkaline non-self-thickening, the problem of thickening of acrylic emulsion in an alkaline environment is solved, the stability of the emulsion and the waterproof and oil-proof performance are improved, and its application scenarios are expanded.
Patent Information
- Application Number
- CN202311202005.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-18
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-09-18
Smart Images

Figure CN117264124B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic coatings, and in particular relates to a method for preparing an alkali-insensitive self-thickening gradient core-shell acrylic emulsion. Background Art
[0002] Acrylate copolymer emulsion has excellent weather resistance, acid and alkali resistance, scrub resistance and high adhesion, and is widely used in many fields such as textiles, paper products, pressure-sensitive adhesives, coatings and leather processing; with the upgrade of the plastic ban, many paper-over-plastic composite products, plastic synthetic paper and coated paper are gradually being eliminated by the packaging and printing industry because they cannot meet the environmental protection requirements of recyclability, repulpability and biodegradability. Therefore, products coated with functional coatings on paper have become products urgently needed in the market. With the development of modern industrial science and technology, acrylate and copolymer emulsions have been widely used. In the process of synthesizing acrylate emulsions, functional monomers such as acrylic acid or methacrylic acid are usually introduced to make them have an alkali thickening effect, and to regulate the stability of the polymer emulsion, storage stability and the formulation of the later latex paint. But at the same time, unsaturated carboxylic acids also bring limitations to the application scenarios. For environments with slightly higher alkalinity, they will thicken significantly, be difficult to flow, and even clump, which greatly limits the application of the emulsion. Therefore, there is an urgent need for an emulsion that does not thicken in an alkaline environment, has good process stability, storage stability, good compatibility, and has basic oil and water resistance and anti-sticking functions. Summary of the invention
[0003] In view of the problems existing in the prior art, the present invention provides a method for preparing an alkali-insensitive self-thickening gradient core-shell acrylic emulsion.
[0004] In order to solve the above technical problems, the present invention adopts the following technical solution: an alkali-insensitive self-thickening gradient core-shell acrylic emulsion, comprising the following material compositions in weight percentage:
[0005] 30-50 parts of hard monomer
[0006] Soft monomer 45-65 parts
[0007] 2-6 parts of cross-linking monomer
[0008] Functional monomer 1-3 copies
[0009] Silane coupling agent 0.5-1.2 parts
[0010] 1.5-2.2 parts of polymerizable emulsifier
[0011] Initiator 0.2-1 part
[0012] Oxidant 0.2-0.6 parts
[0013] Reducing agent 0.1-0.3 parts
[0014] Antibacterial agent 0.005-3 parts
[0015] 60-80 parts of deionized water
[0016] The hard monomer is one or more of styrene, methyl methacrylate, tert-butyl methacrylate, and isobornyl methacrylate;
[0017] The soft monomer is one or more of n-butyl acrylate, isooctyl acrylate, lauryl acrylate, lauryl methacrylate, and 2-ethylhexyl acrylate;
[0018] The cross-linking monomer is one or more of ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, polyethylene glycol (400) dimethacrylate, γ-aminopropyl triethoxysilane, hydroxyethyl acrylamide, and hydroxymethyl acrylamide;
[0019] The polymerizable emulsifier is ammonium allyl fatty alcohol sulfate and / or sodium allyl fatty alcohol sulfate.
[0020] Preferably, the functional monomer is one or more of acrylic acid, methacrylic acid, itaconic acid, hydroxyethyl methacrylate, and hydroxypropyl methacrylate.
[0021] Preferably, the silane coupling agent is one or more of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, and γ(methacryloyloxy)propyltrimethoxysilane.
[0022] Preferably, the oxidizing agent is tert-butyl hydroperoxide; the reducing agent is one or more of ascorbic acid, isoascorbic acid, bleaching agent, sodium sulfite, and Brüggemann FF6M.
[0023] Preferably, the initiator is one or more of potassium persulfate and ammonium persulfate; the fungicide is one or more of methylisothiazolinone and 1,2-benzisothiazolin-3-one.
[0024] Preferably, the composition comprises the following components in parts by weight: 25-40 parts of n-butyl acrylate, 15-25 parts of isooctyl acrylate, 8-12 parts of lauryl methacrylate, 18-22 parts of methyl methacrylate, 15-20 parts of styrene, 1-2 parts of PEG (400) DMA, 4-7 parts of diethylene glycol methacrylate, 3-5 parts of methacrylic acid, 1-3 parts of hydroxypropyl methacrylate, 1.5-2.2 parts of polymerizable emulsifier, 0.2-1 parts of initiator, 0.005-0.3 parts of antibacterial agent and 60-80 parts of deionized water.
[0025] The present invention also provides a method for preparing the above-mentioned alkali non-self-thickening gradient core-shell acrylic emulsion, comprising the following steps:
[0026] Step S1, preparation of pre-emulsion:
[0027] Core layer pre-emulsion: 12-20 parts of hard monomer, 12-20 parts of soft monomer, 0.8-1.5 parts of cross-linking monomer, 3-6 parts of functional monomer and 0.1-0.3 parts of polymerizable emulsifier are added into deionized water, and emulsified in a high-speed homogenizing emulsifier to obtain core layer pre-emulsion;
[0028] Transition layer pre-emulsion: 1-3 parts of hard monomer and 5-10 parts of soft monomer are added to deionized water, and emulsified in a high-speed homogenizing emulsifier to obtain a transition layer pre-emulsion;
[0029] Shell pre-emulsion: 18-25 parts of hard monomer, 30-50 parts of soft monomer, 3-5 parts of cross-linking monomer, 1-2 parts of functional monomer and 0.3-0.6 parts of polymerizable emulsifier are added into deionized water, and emulsified in a high-speed homogenizing emulsifier to obtain shell pre-emulsion;
[0030] Step S2, preparation of kettle bottom liquid: add an appropriate amount of polymerizable emulsifier to deionized water, stir and dissolve to obtain kettle bottom liquid, which is set aside; in addition, add 0.2-0.6 parts of initiator to deionized water, stir and dissolve to prepare an initiator solution, which is set aside;
[0031] Step S3, core emulsion polymerization: the bottom liquid of the kettle is heated to 80±3°C under stirring, and then part of the initiator solution is added thereto, and the temperature is kept for at least 15 minutes; then, the core layer pre-emulsion liquid obtained in step S2 is added dropwise to the reactor at a stirring speed of 150-200 rpm, and the dropping time is controlled to be 1.5-2.5 hours. After the dropping is completed, an appropriate amount of ammonia water is added to neutralize and stir evenly;
[0032] Step S4, then, adding the transition layer pre-emulsion and the initiator into the reactor in a dropwise manner, and the dropping time is controlled within 0.5-1h;
[0033] Step S5, shell emulsion polymerization: continue to add the shell pre-emulsion obtained in step S1 and the remaining initiator solution to the reaction system in a dropwise manner, and control the addition to be completed within 1.5-2.5 hours; after the addition is completed, keep the temperature at 80±3°C for 1-2 hours; then, simultaneously add the oxidant and the reductant to the reaction system within 40±10 minutes, and keep the temperature for 30-50 minutes;
[0034] Step S6, then, continue to heat up to 85±3° C. and keep warm for at least 1 hour, then cool down to below 40° C., add fungicide, and stir evenly to obtain an alkali-free self-thickening gradient core-shell acrylic emulsion with a slightly white-blue appearance.
[0035] Furthermore, the mass fractions of the components of the core layer pre-emulsion are as follows: 10 parts of methyl methacrylate, 5 parts of styrene, 15 parts of butyl acrylate, 1 part of polyethylene glycol (400) dimethacrylate, 4 parts of methacrylic acid and 0.2 parts of a polymerizable emulsifier;
[0036] The mass fractions of the components of the transition layer emulsion are as follows: 2 parts of styrene and 8 parts of isooctyl acrylate;
[0037] The mass fractions of the components of the shell pre-emulsion are as follows: 10 parts of styrene, 10 parts of methyl methacrylate, 20 parts of butyl acrylate, 10 parts of isooctyl acrylate, 5 parts of lauryl methacrylate, 4 parts of diethylene glycol methacrylate, 1.5 parts of hydroxypropyl methacrylate and 0.4 parts of a polymerizable emulsifier.
[0038] Beneficial effects: Compared with the prior art, the present invention has the following advantages:
[0039] 1. Through the design of a non-nucleated transition layer, the emulsion forms a core-shell gradient structure with a certain gradient, so that the carboxylic acid-rich emulsion system can still be stably stored without thickening in an alkaline environment, greatly improving the universality of its formula application scenarios.
[0040] 2. By using internal cross-linking monomers and core-shell functional hydrophilic monomers, a three-dimensional spatial structure is formed between the core and shell, which improves its anti-stickiness and water and oil resistance levels. In addition, through the further differentiated design of the hard core and soft shell of the core-shell structure, it has anti-stick properties and excellent water and oil resistance levels.
[0041] 3. The formulation process is simple, the cost is low, the emulsion has high stability, excellent waterproof and oil-proof properties, can be produced and scaled up repeatedly, and has good compatibility and universality, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the following briefly introduces the drawings required for describing the embodiment, wherein:
[0043] Figure 1 This is the infrared spectrum of the alkali-free self-thickening gradient core-shell acrylic emulsion of the embodiment of the present invention;
[0044] Figure 2 This is a differential scanning calorimetry curve of the alkali-free self-thickening gradient core-shell acrylic emulsion of an embodiment of the present invention;
[0045] Figure 3 The particle size and distribution diagram of the alkali-free self-thickening gradient core-shell acrylic emulsion of the embodiment of the present invention;
[0046] Figure 4 This is a microstructure diagram of the alkali-free self-thickening gradient core-shell acrylic emulsion latex particles of the embodiment of the present invention. DETAILED DESCRIPTION
[0047] The present invention is further illustrated below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. After reading the present invention, modifications to various equivalent forms of the present invention by those skilled in the art all fall within the scope defined by the appended claims of the present application.
[0048] Description of the relationship between the Chinese names and English abbreviations of the substances involved in the present invention:
[0049]
[0050] 1. Preparation of alkali-free self-thickening gradient core-shell acrylic emulsion
[0051] Example 1
[0052] Step S1, preparation of pre-emulsion:
[0053] Core layer pre-emulsion: 10 parts of methyl methacrylate, 5 parts of styrene, 15 parts of butyl acrylate, 4 parts of methacrylic acid and 0.2 parts of a polymerizable emulsifier are added to deionized water, and emulsified in a high-speed homogenizing emulsifier to obtain a core layer pre-emulsion;
[0054] Transition layer pre-emulsion: 2 parts of methyl methacrylate and 8 parts of butyl acrylate are added into deionized water, and emulsified in a high-speed homogenizing emulsifier to obtain a transition layer pre-emulsion;
[0055] Shell pre-emulsion: 10 parts of styrene, 10 parts of methyl methacrylate, 20 parts of butyl acrylate, 10 parts of isooctyl acrylate, 5 parts of lauryl methacrylate and 0.4 parts of a polymerizable emulsifier are added into deionized water and emulsified in a high-speed homogenizing emulsifier to obtain a shell pre-emulsion;
[0056] Step S2, preparation of kettle bottom liquid: add an appropriate amount of polymerizable emulsifier to deionized water, stir and dissolve to obtain kettle bottom liquid, which is set aside; in addition, add 0.2-0.6 parts of initiator to deionized water, stir and dissolve to prepare an initiator solution, which is set aside;
[0057] Step S3, core emulsion polymerization: the bottom liquid of the kettle is heated to 80±3°C under stirring, and then part of the initiator solution is added thereto, and the temperature is kept for at least 15 minutes; then, the core layer pre-emulsion liquid obtained in step S2 is added dropwise to the reactor at a stirring speed of 150-200 rpm, and the dropping time is controlled to be 1.5-2.5 hours. After the dropping is completed, an appropriate amount of ammonia water is added to neutralize and stir evenly;
[0058] Step S4, then, adding the transition layer pre-emulsion and the initiator into the reactor in a dropwise manner, and the dropping time is controlled within 0.5-1h;
[0059] Step S5, shell emulsion polymerization: continue to add the shell pre-emulsion obtained in step S1 and the remaining initiator solution to the reaction system in a dropwise manner, and control the addition to be completed within 1.5-2.5 hours; after the addition is completed, keep the temperature at 80±3°C for 1-2 hours; then, simultaneously add the oxidant and the reductant to the reaction system within 40±10 minutes, and keep the temperature for 30-50 minutes;
[0060] Step S6, then, continue to heat up to 85±3° C. and keep warm for at least 1 hour, then cool down to below 40° C., add fungicide, and stir evenly to obtain a milky white alkali-free self-thickening gradient core-shell acrylic emulsion.
[0061] Embodiment 2-9
[0062] Compared with Example 1, the difference of this example is that the types and addition amounts of the reaction materials are different, as shown in Table 1-3 for details.
[0063] Table 1 shows the addition amount of each component of the core layer pre-emulsion in each embodiment.
[0064]
[0065] Table 2 shows the addition amount of each component of the transition layer premix in each embodiment.
[0066]
[0067] Table 3 shows the addition amount of each component of the shell pre-emulsion in each embodiment.
[0068]
[0069] The alkali-free self-thickening gradient core-shell acrylic emulsion obtained in each example was prepared into a cured film according to the following method to test various properties:
[0070] 2. Performance Test
[0071] Preparation of cured film: Use OSP-15 or OSP-18# wire rod to coat the test paper (Golden Sun 210g / m2 uncoated food base paper, size 10cm*5cm), with a coating dry weight of about 5-7g / ㎡, and number them according to the example serial number. Then put the test paper samples into an oven set at 120°C, and place the paper samples for 50 seconds to cure into films.
[0072] (1) Viscosity test: The viscosity η0 of each sample at room temperature was measured using a 4-cup coating. Each sample was then neutralized to pH 9 using 10% ammonia water and placed at room temperature for 6 months. The thickening viscosity η was measured. The test found that the viscosity changed very little, which was 5-6 times smaller than that of the non-gradient core-shell structure.
[0073] (2) Water resistance test: According to GB / T1540-2002 "Determination of water absorption of paper and paperboard (COBB method)", the water resistance is measured using a COBB absorbency meter. The core-shell acrylic emulsion obtained in Examples 1 to 3 of the present invention is prepared into a water-based barrier coating, and the COBB value is <3, which is close to the water-releasing effect of PE coating, and can meet the waterproof requirements in normal use scenarios.
[0074] In addition, the present invention also uses the following more intuitive method for detection: take a paper sample coated with barrier resin prepared according to the above method, fold and stick a sample box with a bottom side length of 100 mm and a height of 50 mm, and place it flat on a dry glass plate or flat plate lined with filter paper. Pour hot water with a temperature of (95±5)℃ into the sample box, add water to a liquid level of 40mm, let it stand for 30 minutes, and observe whether there is a watermark on the filter paper lining the glass plate or flat plate. 3 samples are measured for each sample.
[0075] (3) Oil resistance test: refer to the requirements of GB / T22805.2-2008 "Determination of fat resistance of paper and paperboard" Part 2: Surface removal method and T / ZZB 1448-2019 "White oil-proof paper for food packaging" for oil resistance test. The oil resistance level is required to be ≥ 9, and the highest is 12. The method is as follows: test with kit standard oil, and the sample paper coated with the barrier resin prepared by the core-shell acrylic emulsion listed in Examples 1 to 3 of the present invention can achieve oil resistance level 10 without loss of gloss and level 12 without leakage, which can meet most of the oil resistance performance requirements. In addition, the present invention also uses the following more intuitive method for detection: take a paper sample coated with barrier resin prepared according to the above method, fold and glue a sample box with a bottom side length of 100 mm and a height of 50 mm, and place it flat on a dry glass plate or flat plate lined with filter paper. Pour hot oil at a temperature of (95±5)℃ into the sample box, add oil to a liquid level of 40mm, let it stand for 30 minutes, and observe whether there is oil seepage on the filter paper on the dry glass plate or flat plate. During the test, the oil may seep upward along the sample. Make sure there is no oil on the upper port of the sample box, otherwise the oil may seep out from the upper port and affect the test results. Measure 3 samples for each sample.
[0076] (4) Anti-heat-adhesion test: Take a paper sample coated with barrier resin prepared according to the above method, cut it into square pieces of 5 cm in length and width, and stack them together with the coating surface facing the coating surface (face to face) and the back of the paper facing the coating surface (back to back). Press them with a 5 kg weight and bake them in a 60 ° C oven for 6 hours. After cooling, both the face-to-face and back-to-back surfaces can fall off naturally, which can meet the high anti-heat-adhesion requirements of the barrier coating.
[0077] Through the above tests, the test results of the cured film properties of each embodiment were obtained, as shown in Table 4.
[0078] Table 4 is the test results of the cured film properties obtained in each embodiment
[0079]
[0080] From the test results of each embodiment, it can be seen that:
[0081] Example 1: Without using a cross-linking monomer, the emulsion can have good water and oil resistance, but poor anti-adhesion. The presence of the transition layer will prevent the emulsion from self-thickening in an alkaline environment, but the emulsion itself is whitish and has poor storage stability.
[0082] Examples 2 and 3: By comparing Examples 2 and 3, it can be found that the combination of two soft and hard monomers with large steric hindrance, isooctyl acrylate and styrene, in the transition layer can make the transition layer more stable through the restriction of steric hindrance, making the emulsion state slightly white and bluish and more stable.
[0083] Example 4: It can be found from Example 4 that the pre-emulsified addition of the monomers in the transition layer will cause secondary nucleation between the core-shell system to form an irregular three-layer heterogeneous structure, which will reduce the water and oil resistance of the emulsion and aggravate the self-thickening effect in an alkaline environment.
[0084] Examples 5, 6 and 7: By comparing Examples 5, 6 and 7, it can be found that the use of internal cross-linking monomers in the core layer, transition layer and shell layer respectively / simultaneously can form an interwoven three-dimensional network space structure between molecules, limit the rotation of bonds and the slip of chain segments, and thus have a better anti-stick effect. However, the use of cross-linking monomers in the transition layer will reduce the waterproof and oil-proof properties of the emulsion.
[0085] Examples 8 and 9: By comparing Examples 8 and 9, it can be found that in the absence of a transition layer structure, the self-thickening effect of the emulsion in an alkaline environment is significantly aggravated, so that the emulsion clumps and has no fluidity. The use of a hydroxyl-containing hydroxypropyl methacrylate monomer in the shell layer can, on the one hand, form a hydrophilic gradient difference between the core and shell layers, which is helpful for stabilizing the emulsion system. On the other hand, it can form a micro-cross-linked structure between the core and shell, further enhancing the anti-stick and waterproof effects.
Claims
1. A method for preparing an alkali-free self-thickening gradient core-shell acrylic emulsion, characterized in that The following steps are involved: Step S1, preparation of pre-emulsion: Core layer pre-emulsion: 12-20 parts of hard monomer, 12-20 parts of soft monomer, 0.8-1.5 parts of cross-linking monomer, 3-6 parts of functional monomer and 0.1-0.3 parts of polymerizable emulsifier are added into deionized water, and emulsified in a high-speed homogenizing emulsifier to obtain core layer pre-emulsion; Transition layer pre-emulsion: 1-3 parts of hard monomer and 5-10 parts of soft monomer are added to deionized water, and emulsified in a high-speed homogenizing emulsifier to obtain a transition layer pre-emulsion; Shell pre-emulsion: 18-25 parts of hard monomer, 30-50 parts of soft monomer, 3-5 parts of cross-linking monomer, 1-2 parts of functional monomer and 0.3-0.6 parts of polymerizable emulsifier are added into deionized water, and emulsified in a high-speed homogenizing emulsifier to obtain shell pre-emulsion; Step S2, preparation of kettle bottom liquid: add an appropriate amount of polymerizable emulsifier to deionized water, stir and dissolve to obtain kettle bottom liquid, which is set aside; in addition, add 0.2-0.6 parts of initiator to deionized water, stir and dissolve to prepare an initiator solution, which is set aside; Step S3, core emulsion polymerization: the bottom liquid of the kettle is heated to 80±3°C under stirring, and then part of the initiator solution is added thereto, and the temperature is kept at least 15 minutes; then, the core layer pre-emulsion liquid obtained in step S1 is added to the reactor in a dropwise manner at a stirring speed of 150-200 rpm, and the dropping time is controlled to be 1.5-2.5 hours. After the dropping is completed, an appropriate amount of ammonia water is added to neutralize and stir evenly; Step S4, then, adding the transition layer pre-emulsion and the initiator into the reactor in a dropwise manner, and the dropping time is controlled within 0.5-1h; Step S5, shell emulsion polymerization: continue to add the shell pre-emulsion obtained in step S1 and the remaining initiator solution to the reaction system in a dropwise manner, and control the addition to be completed within 1.5-2.5 hours; after the addition is completed, keep the temperature at 80±3°C for 1-2 hours; then, simultaneously add the oxidant and the reductant to the reaction system within 40±10 minutes, and keep the temperature for 30-50 minutes; Step S6, then, continue to heat up to 85±3° C. and keep warm for at least 1 hour, then cool down to below 40° C., add fungicide, and stir evenly to obtain an alkali-free self-thickening gradient core-shell acrylic emulsion with a slightly white-blue appearance.
2. The method for preparing the alkali-free self-thickening gradient core-shell acrylic emulsion according to claim 1, characterized in that: The functional monomer is one or more of acrylic acid, methacrylic acid, itaconic acid, hydroxyethyl methacrylate, and hydroxypropyl methacrylate.
3. The method for preparing the alkali-free self-thickening gradient core-shell acrylic emulsion according to claim 1, characterized in that: The functional monomer is one or more of acrylic acid, methacrylic acid, itaconic acid, hydroxyethyl methacrylate, and hydroxypropyl methacrylate.
4. The method for preparing the alkali-free self-thickening gradient core-shell acrylic emulsion according to claim 1, characterized in that: The hard monomer is one or more of styrene, methyl methacrylate, tert-butyl methacrylate, and isobornyl methacrylate.
5. The method for preparing the alkali-free self-thickening gradient core-shell acrylic emulsion according to claim 1, characterized in that: The soft monomer is one or more of n-butyl acrylate, isooctyl acrylate, lauryl acrylate, lauryl methacrylate, and 2-ethylhexyl acrylate.
6. The method for preparing the alkali-insensitive self-thickening gradient core-shell acrylic emulsion according to claim 1, characterized in that: The cross-linking monomer is one or more of ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, polyethylene glycol (400) dimethacrylate, γ-aminopropyl triethoxysilane, hydroxyethyl acrylamide, and hydroxymethyl acrylamide.
7. The method for preparing the alkali-insensitive self-thickening gradient core-shell acrylic emulsion according to claim 1, characterized in that: The polymerizable emulsifier is ammonium allyl fatty alcohol sulfate and / or sodium allyl fatty alcohol sulfate.
8. The method for preparing the alkali-insensitive self-thickening gradient core-shell acrylic emulsion according to claim 1, characterized in that: The mass fractions of the components of the core layer pre-emulsion are as follows: the hard monomer is 10 parts of methyl methacrylate and 5 parts of styrene, the soft monomer is 15 parts of butyl acrylate, the cross-linking monomer is 1 part of polyethylene glycol (400) dimethacrylate, and the functional monomer is 4 parts of methacrylic acid and 0.2 parts of a polymerizable emulsifier; The mass fractions of the components of the transition layer emulsion are as follows: 2 parts of hard monomer styrene and 8 parts of soft monomer isooctyl acrylate; the mass fractions of the components of the shell pre-emulsion are as follows: the hard monomer is 10 parts of styrene and 10 parts of methyl methacrylate, the soft monomer is 20 parts of butyl acrylate, 10 parts of isooctyl acrylate, and 5 parts of lauryl methacrylate, the cross-linking monomer is 4 parts of diethylene glycol methacrylate, and the functional monomer is 1.5 parts of hydroxypropyl methacrylate and 0.4 parts of a polymerizable emulsifier.