Self-cleaning film and preparation method thereof and photovoltaic module
By annealing and surface modification of perlite, a self-cleaning film for photovoltaic modules was prepared, which solved the problem of pollution accumulation in the outdoor environment of photovoltaic modules, and achieved the self-cleaning effect and durability of the modules.
Patent Information
- Application Number
- CN202311240787.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-25
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-09-25
AI Technical Summary
Traditional photovoltaic modules are easily accumulated by dust, rainwater and other pollutants in outdoor environments, resulting in reduced heat generation, light transmittance and reduced power. At the same time, seawater and acid rain will corrode the aluminum frame, affecting the reliability of the components.
By annealing and surface modification of perlite, a self-cleaning film with good hydrophobic properties was prepared, combined with acrylic resin as a substrate, the mechanical strength and environmental tolerance were improved, and the film layer could be automatically cleaned was formed.
The self-cleaning effect of photovoltaic module surfaces is achieved, which improves light transmittance and efficiency, avoids frame corrosion, and improves the long-term reliability and durability of the module.
Smart Images

Figure CN117264489B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photovoltaic modules, in particular to a self-cleaning film and a preparation method thereof, and a photovoltaic module. Background Art
[0002] Self-cleaning membranes include hydrophobic self-cleaning membranes and hydrophilic self-cleaning membranes. They are a type of membrane layer that can achieve automatic surface cleaning. The principle is that water slides down the surface after falling on it, and takes away the dust on the surface, thereby achieving self-cleaning. However, due to the harshness of the outdoor environment, the traditional technology uses surface hydrophobic modification on perlite, but its self-cleaning effect, environmental tolerance and mechanical strength still cannot meet the use requirements. For example, when photovoltaic modules work outdoors for a long time, pollutants such as dust and rain will accumulate on the glass surface of the module, causing heating of the module, reduced light transmittance, reduced power and other problems. At the same time, seawater and acid rain will corrode the aluminum frame of the module, seriously affecting the reliability of the module. Summary of the invention
[0003] Based on this, it is necessary to provide a self-cleaning film and its preparation method and photovoltaic module. The self-cleaning film adopts annealing modified perlite material to effectively improve the hydrophobicity and uses acrylic resin as the base material, and has the characteristics of good environmental tolerance and high mechanical strength.
[0004] The above-mentioned object of the invention can be achieved through the following technical solutions.
[0005] In a first aspect, the present application provides a method for preparing a self-cleaning membrane, the preparation method comprising:
[0006] The annealed perlite is subjected to surface modification to obtain modified perlite;
[0007] The modified perlite, acrylic resin and solvent are mixed and then coated to obtain the self-cleaning film.
[0008] In some embodiments, the annealing treatment is performed at a temperature of 300° C. to 550° C. and for a time of 0.5 h to 1.5 h.
[0009] In some embodiments, the annealing treatment is performed in a protective atmosphere.
[0010] Optionally, the protective atmosphere includes at least one of an inert gas and nitrogen.
[0011] In some embodiments, the perlite is present in an amount of 30 to 95 parts by mass.
[0012] In some embodiments, the acrylic resin is present in an amount of 1 to 19 parts by mass.
[0013] In some embodiments, the solvent is present in an amount of 4 to 76 parts by mass.
[0014] In some embodiments, the particle size of the perlite is 10 μm to 50 μm.
[0015] In some embodiments, the perlite is ground prior to the annealing process.
[0016] In some embodiments, the perlite has a plate-like structure and a block-like structure.
[0017] In some embodiments, the surface modification method comprises:
[0018] The annealed perlite is mixed with a surfactant to form a solution, and the solution is dried to obtain the modified perlite.
[0019] In some embodiments, the surfactant comprises a silanol.
[0020] In some embodiments, the mass of the surfactant is 5% to 9% of the mass of the perlite.
[0021] In some embodiments, the surfactant is present in an amount of 0.35 parts to 6.65 parts by mass.
[0022] In some embodiments, the acrylic resin includes at least one of isobutyl methacrylate / styrene resin, butyl acrylate resin, methacrylate resin, methyl methacrylate resin, and methyl methacrylate / styrene resin.
[0023] In some embodiments, the solvent comprises xylene.
[0024] In a second aspect, the present application provides a self-cleaning film, which is prepared by the method for preparing a self-cleaning film as described in the first aspect, and comprises an acrylic resin substrate layer and modified perlite dispersed in the acrylic resin substrate layer.
[0025] In some embodiments, the self-cleaning film has a thickness of 0.01 mm to 1 mm.
[0026] In a third aspect, the present application provides a photovoltaic module, wherein the photovoltaic module comprises the self-cleaning film as described in the second aspect.
[0027] Compared with the traditional technology, this application has at least the following beneficial effects:
[0028] The present application performs annealing and surface modification on perlite, thereby reducing the surface energy of the perlite material and improving the hydrophobicity of the self-cleaning membrane; and after annealing, the perlite increases the proportion of perlite flaky structures, improves the surface roughness of the material and the gas-liquid contact surface, and reduces the surface energy of the material itself, improving the surface modification ability of the perlite. When water falls on the self-cleaning material layer of the present application, it can quickly pass through the surface of the self-cleaning material layer, while taking away dust and other pollutants on the surface, achieving the effect of self-cleaning of the component, and has the characteristics of good environmental tolerance and high mechanical strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is an optical microscope image of the surface of the self-cleaning membrane provided in Example 1 of the present application.
[0030] Figure 2 This is an internal optical microscope image of the self-cleaning membrane provided in Example 1 of the present application.
[0031] Figure 3 This is a graph showing the change in contact angle of the self-cleaning film as a function of friction intensity provided in Example 1 of the present application.
[0032] Figure 4 This is a graph showing the change in contact angle of the self-cleaning membrane provided in Example 1 of the present application during the soaking time in water.
[0033] Figure 5 This is an optical microscope image of the untreated perlite in Example 1 of the present application.
[0034] Figure 6 This is an optical microscope image of the perlite after grinding treatment in Example 1 of the present application.
[0035] Figure 7 This is an optical microscope image of the perlite after annealing in Example 1 of the present application. DETAILED DESCRIPTION
[0036] The present invention is further described in detail below in conjunction with the accompanying drawings, embodiments and examples. These embodiments and examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. The purpose of providing these embodiments and examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive. It should also be understood that the present invention can be implemented in many different forms and is not limited to the embodiments and examples described herein. Those skilled in the art can make various changes or modifications without violating the connotation of the present invention, and the equivalent forms obtained also fall within the protection scope of the present invention. In addition, in the following description, a large number of specific details are given in order to provide a more comprehensive understanding of the present invention. It should be understood that the present invention can be implemented without one or more of these details.
[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0038] In the present invention, "optionally", "optional", and "optional" mean optional, that is, any one of the two parallel solutions of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0039] In the present invention, the terms "first", "second", "third", etc. in "the first aspect", "the second aspect", "the third aspect", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0040] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0041] In the present invention, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values in the numerical interval is considered to be continuous, and includes the two numerical endpoints (i.e., the minimum value and the maximum value) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to the integers in the numerical interval, including the two endpoint integers of the numerical range, and each integer between the two endpoints, is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined. In other words, unless otherwise specified, the numerical ranges disclosed in this application should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows for broadly including quantitative intervals such as percentage intervals, ratio intervals, and ratio intervals.
[0042] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as a reference separately. Unless they conflict with the invention purpose and / or technical solution of the present application, the cited documents involved in the present invention are cited with all contents and all purposes. When the present invention involves cited documents, the definitions of relevant technical features, terms, nouns, phrases, etc. in the cited documents are also cited. When the present invention involves cited documents, the examples and preferred embodiments of the cited relevant technical features may also be incorporated into this application as references, but are limited to the ability to implement the present invention. It should be understood that when the content of the citation conflicts with the description in this application, the present application shall prevail or be modified adaptively according to the description of this application.
[0043] During the use of photovoltaic modules, pollutants are easily left on their surface, which in turn affects the surface transmittance of the modules. In addition, photovoltaic modules may be corroded in seawater or acid rain environments. In this application, the self-cleaning material layer prepared by annealing and surface modification of perlite has the characteristics of good hydrophobicity, good wear resistance and excellent blister resistance. When water falls on the surface of the self-cleaning material layer, it can quickly flow away and take away surface pollutants.
[0044] The first aspect of the present application provides a method for preparing a self-cleaning membrane, the preparation method comprising:
[0045] The annealed perlite is subjected to surface modification to obtain modified perlite;
[0046] The modified perlite, acrylic resin and solvent are mixed and then coated to obtain the self-cleaning film.
[0047] The present application first anneals the perlite, and the annealing process can increase the proportion of the flaky perlite structure, and the flaky perlite is arranged in a parallel, vertical or intersecting manner, thereby improving the surface roughness and gas-liquid contact surface of the material. Furthermore, the annealing process can remove organic impurities in the perlite, reduce the surface energy of the material and improve the surface modification effect of the perlite, thereby improving the surface modification reaction, reducing the surface energy of the material, and effectively improving the hydrophobic properties of the self-cleaning film during the surface modification process. Moreover, the self-cleaning film of the present application has excellent wear resistance and blister resistance.
[0048] It should be noted that perlite refers to glassy, transparent, colorless, and has an expansion multiple of more than 20. Specifically, the perlite includes 68% to 74% SiO2, 11% to 13% Al2O3, 0.5% to 3.6% Fe2O3, 0.7% to 1.0% CaO, 2% to 3% K2O, 4% to 5% Na2O, 0.2% to 0.4% MgO, and 2.3% to 6.4% H2O.
[0049] In some embodiments, the annealing temperature is 300°C to 550°C, for example, 300°C, 320°C, 340°C, 360°C, 380°C, 400°C, 420°C, 440°C, 460°C, 480°C, 500°C, 520°C, 540°C or 550°C.
[0050] The present application controls the temperature of the annealing treatment, removes the organic components in the perlite, increases the proportion of the flaky structure in the perlite, and improves the surface modification effect. If the annealing temperature is low, the organic components may not be completely removed, resulting in a decrease in the hydrophobicity of the material; if the annealing temperature is high, the microstructure of the perlite material may be affected, thereby affecting the surface energy of the material.
[0051] Optionally, the annealing treatment time is 0.5h to 1.5h, for example, it can be 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1.0h, 1.1h, 1.2h, 1.3h, 1.4h or 1.5h.
[0052] In some embodiments, the annealing treatment is performed in a protective atmosphere. It is understood that the protective atmosphere refers to a gas that does not react with the raw material.
[0053] Optionally, the protective atmosphere includes at least one of an inert gas and nitrogen. For example, the inert gas may be argon.
[0054] In some embodiments, after the annealing treatment, the perlite with a flaky structure accounts for 70% to 90% of the total mass of the perlite, for example, it can be 70%, 72%, 74%, 76%, 78%, 80%, 82%, 84%, 86%, 88% or 90%.
[0055] In some embodiments, the perlite is 30 to 95 parts by weight, for example, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90 or 95 parts. Preferably, it is 75 to 95 parts.
[0056] In some embodiments, the acrylic resin is present in an amount of 1 to 19 parts by weight, for example, 1 part, 2 parts, 4 parts, 6 parts, 8 parts, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts or 19 parts.
[0057] In some embodiments, the solvent is 4 to 76 parts by mass, for example, 4, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75 or 76 parts.
[0058] In some embodiments, the particle size of the perlite is 10 μm to 50 μm, for example, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 32 μm, 34 μm, 36 μm, 38 μm, 40 μm, 42 μm, 44 μm, 46 μm, 48 μm or 50 μm. It is understood that the smaller the particle size of the perlite, the better the hydrophobic property.
[0059] In some embodiments, the perlite is ground prior to the annealing process.
[0060] In the present application, the perlite is ground before annealing. The grinding process can arrange the perlite with flaky or blocky structures in parallel, vertical or intersecting order, thereby increasing the surface roughness of the material and increasing the gas-liquid contact area.
[0061] In some embodiments, the perlite is washed with an organic solvent to remove organic impurities after the grinding process, and then annealed.
[0062] Optionally, the organic solvent includes sunflower oil. Further optionally, the mass ratio of the perlite to the organic solvent is (1.5-2.5):1, preferably 2:1.
[0063] In some embodiments, the perlite has a flaky structure and a blocky structure. It should be noted that the flaky structure refers to perlite with a thickness of 0 to 10 μm, and the blocky structure refers to perlite with a thickness greater than 10 μm.
[0064] It should be noted that the perlite in the present application can be obtained by grinding expanded perlite, and the expanded perlite refers to perlite with a hollow microsphere structure and a particle size of 100 μm to 700 μm.
[0065] In some embodiments, the surface modification method comprises:
[0066] The annealed perlite is mixed with a surfactant to form a solution, and the solution is dried to obtain the modified perlite.
[0067] In some embodiments, the solvent in the solution may be ultrapure water.
[0068] In some embodiments, the surfactant includes a silanol. For example, the silanol includes at least one of trimethylsilanol, polydiethylsilanol and triethylsilanol. In the present application, a silanol fluid is used as a surface modifier, and its molecular structure has active chemical bonds, thereby having good film-forming properties.
[0069] In some embodiments, the mass of the surfactant is 5% to 9% of the mass of the perlite, for example, 5.0%, 5.4%, 5.8%, 6.2%, 6.6%, 7.0%, 7.4%, 7.8%, 8.2%, 8.6% or 9.0%.
[0070] The present application controls the quality of the surfactant, reduces the surface energy of the perlite material, and improves the hydrophobicity. If the quality is relatively low, the surface modification of the perlite may be incomplete, affecting the reduction of the surface energy and poor hydrophobicity; if the quality is relatively high, it may cause the surfactant to remain, thereby affecting the hydrophobicity of the self-cleaning film formed by the modified perlite.
[0071] In some embodiments, the surfactant is 0.35 to 6.65 parts by mass, for example, it can be 0.35, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5 or 6.65 parts.
[0072] In some embodiments, the acrylic resin includes at least one of isobutyl methacrylate / styrene resin, butyl acrylate resin, methacrylate resin, methyl methacrylate resin and methyl methacrylate / styrene resin. Preferably, it is isobutyl methacrylate / styrene resin, which refers to a mixture of isobutyl methacrylate and styrene resin, and the mass ratio of isobutyl methacrylate to styrene resin is 1:1.
[0073] Isobutyl methacrylate / styrene is a transparent, non-toxic thermoplastic resin with good processing fluidity and low hygroscopicity, excellent weather resistance and impact strength, excellent optical properties and light transmittance. Isobutyl methacrylate / styrene protects the hydrophobic base layer in the coating system, providing the coating with excellent weather resistance, excellent optical properties and light transmittance.
[0074] In some embodiments, the solvent includes xylene. Optionally, the xylene includes at least one of meta-xylene, para-xylene and o-xylene. Further optionally, the xylene includes 45% to 70% meta-xylene, 15% to 25% para-xylene and 10% to 15% o-xylene. Xylene is used as a solvent for acrylic resin in the system to fully dissolve the acrylic resin and fully mix it with perlite.
[0075] Exemplarily, a method for preparing the self-cleaning film is provided, comprising:
[0076] Grinding the perlite, wherein the particle size of the perlite after the grinding process is 10 μm to 50 μm, adding an organic solvent to the ground perlite, and the mass ratio of the perlite to the organic solvent is (1.5 to 2.5):1;
[0077] The cleaned perlite is placed in a muffle furnace and annealed at 300°C to 550°C for 0.5h to 1.5h under a protective atmosphere; the annealed perlite is then mixed with a surfactant and dried to obtain a modified perlite, wherein the mass of the surfactant is 5% to 9% of the mass of the perlite;
[0078] The modified perlite, acrylic resin and solvent are mixed and then coated to obtain the self-cleaning film.
[0079] The second aspect of the present application provides a self-cleaning film, which is prepared by the method for preparing a self-cleaning film as described in the first aspect. The self-cleaning film includes an acrylic resin substrate layer and modified perlite dispersed on the surface of the acrylic resin substrate layer.
[0080] It is understood that part of the modified perlite protrudes from the surface of the acrylic resin substrate layer.
[0081] In some embodiments, the self-cleaning film has a thickness of 0.01 mm to 1 mm, for example, 0.01 mm, 0.05 mm, 0.10 mm, 0.20 mm, 0.30 mm, 0.40 mm, 0.50 mm, 0.60 mm, 0.70 mm, 0.80 mm, 0.90 mm or 1.00 mm.
[0082] A third aspect of the present application provides a photovoltaic module, wherein the photovoltaic module comprises the self-cleaning film as described in the second aspect.
[0083] In this application, the self-cleaning film is applied to photovoltaic modules. When water falls on the photovoltaic modules, it can quickly pass through the module surface and take away dust and other pollutants on the module surface, thereby achieving the effect of self-cleaning of the module, improving the light transmittance of the surface glass, and avoiding heating of the photovoltaic module due to pollutants, thereby improving the efficiency and reliability of the photovoltaic module. In addition, in seawater or acid rain environments, water quickly passes through the module frame to avoid frame corrosion and improve the long-term reliability of the photovoltaic module.
[0084] In some embodiments, the self-cleaning film is disposed on a surface of the photovoltaic component.
[0085] The self-cleaning film is used in the photovoltaic module of the present application to achieve the effect of self-cleaning, improve the light transmittance of the glass on the surface of the module, avoid frame corrosion, and improve the efficiency and long-term reliability of the module. At the same time, the self-cleaning film has a simple formula, low cost, strong cleaning ability, and high environmental tolerance.
[0086] The embodiments of the present invention will be described in detail below in conjunction with examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are preferably referred to the guidance provided in the present invention, and can also be based on the experimental manual or normal conditions in this area, can also be based on the conditions recommended by the manufacturer, or refer to experimental methods known in the art.
[0087] In the following examples and comparative examples, perlite was purchased from Xinyang Juncheng Mining Co., Ltd., with an average particle size of 500 μm; the solvent used was xylene, which was a mixture of 65% m-xylene, 20% p-xylene and 15% o-xylene; the acrylic resin used was isobutyl methacrylate / styrene resin ( B-880), surface modifiers using silanol fluid (XIAMETER TM PMX-0156, mainly including trimethylsilanol); sunflower oil was purchased from Weiqi Biotechnology Co., Ltd.
[0088] Example 1
[0089] Weigh the raw materials according to mass fraction, including:
[0090] 75 parts of perlite, 5.25 parts of surface modifier, 20 parts of xylene, 5 parts of isobutyl methacrylate / styrene; wherein the mass of the surfactant is 7% of the mass of the perlite;
[0091] Grinding the perlite to obtain a particle size of 40 μm, adding sunflower oil to the ground perlite, and the mass ratio of the perlite to the sunflower oil is 2:1;
[0092] The cleaned perlite is placed in a muffle furnace and annealed at 400° C. for 1 hour in a nitrogen atmosphere; the annealed perlite is then mixed with a surfactant and dried to obtain modified perlite;
[0093] After the modified perlite, acrylic resin and solvent are mixed, the self-cleaning film is coated to obtain a thickness of 0.1 mm. The surface structure of the self-cleaning film is as follows: Figure 1 As shown, the internal structure is as Figure 2 shown.
[0094] Example 2
[0095] Weigh the raw materials according to mass fraction, including:
[0096] 75 parts of perlite, 3.75 parts of surface modifier, 20 parts of xylene, 5 parts of isobutyl methacrylate / styrene; wherein the mass of the surfactant is 5% of the mass of the perlite;
[0097] Grinding the perlite to obtain a particle size of 50 μm, adding sunflower oil to the ground perlite, and the mass ratio of the perlite to the sunflower oil is 2:1;
[0098] The cleaned perlite is placed in a muffle furnace and annealed at 550° C. for 0.5 h in a nitrogen atmosphere; the annealed perlite is then mixed with a surfactant and dried to obtain modified perlite;
[0099] After the modified perlite, acrylic resin and solvent are mixed, the self-cleaning film having a thickness of 0.5 mm is coated.
[0100] Example 3
[0101] Weigh the raw materials according to mass fraction, including:
[0102] 50 parts of perlite, 4.5 parts of surface modifier, 31 parts of xylene, 19 parts of isobutyl methacrylate / styrene; wherein the mass of the surfactant is 9% of the mass of the perlite;
[0103] Grinding the perlite to obtain a particle size of 10 μm, adding sunflower oil to the ground perlite, and the mass ratio of the perlite to the sunflower oil is 2:1;
[0104] The cleaned perlite is placed in a muffle furnace and annealed at 300° C. for 1.5 h in a nitrogen atmosphere; the annealed perlite is then mixed with a surfactant and dried to obtain modified perlite;
[0105] The modified perlite, acrylic resin and solvent are mixed and then coated to obtain the self-cleaning film with a thickness of 1 mm.
[0106] Example 4
[0107] The self-cleaning membrane was prepared according to the method of Example 1, except that the raw material contents were different, including:
[0108] 85 parts of perlite, 5.95 parts of surface modifier, 12 parts of xylene, and 3 parts of isobutyl methacrylate / styrene; wherein the mass of the surfactant is 7% of the mass of the perlite.
[0109] Example 5
[0110] The self-cleaning membrane was prepared according to the method of Example 1, except that the raw material contents were different, including:
[0111] 65 parts of perlite, 4.55 parts of surface modifier, 28 parts of xylene, and 7 parts of isobutyl methacrylate / styrene; wherein the mass of the surfactant is 7% of the mass of the perlite.
[0112] Example 6
[0113] The self-cleaning membrane was prepared according to the method of Example 1, except that the raw material contents were different, including:
[0114] 55 parts of perlite, 3.85 parts of surface modifier, 36 parts of xylene, and 9 parts of isobutyl methacrylate / styrene; wherein the mass of the surfactant is 7% of the mass of the perlite.
[0115] Example 7
[0116] The self-cleaning membrane was prepared according to the method of Example 1, except that the raw material contents were different, including:
[0117] 45 parts of perlite, 3.15 parts of surfactant, 44 parts of xylene, and 11 parts of isobutyl methacrylate / styrene; wherein the mass of the surfactant is 7% of the mass of the perlite.
[0118] Example 8
[0119] The self-cleaning membrane was prepared according to the method of Example 1, except that the raw material contents were different, including:
[0120] 35 parts of perlite, 2.45 parts of surfactant, 52 parts of xylene, and 13 parts of isobutyl methacrylate / styrene; wherein the mass of the surfactant is 7% of the mass of the perlite.
[0121] Example 9
[0122] A self-cleaning membrane was prepared according to the method of Example 1, except that the temperature of the annealing treatment was 250°C.
[0123] Example 10
[0124] A self-cleaning membrane was prepared according to the method of Example 1, except that the temperature of the annealing treatment was 600°C.
[0125] Embodiment 11
[0126] A self-cleaning film was prepared according to the method of Example 1, except that the amount of surfactant added was adjusted so that the mass of the surfactant was 3% of the mass of the perlite.
[0127] Example 12
[0128] A self-cleaning film was prepared according to the method of Example 1, except that the amount of surfactant added was adjusted so that the mass of the surfactant was 12% of the mass of the perlite.
[0129] Comparative Example 1
[0130] A self-cleaning membrane was prepared according to the method of Example 1, except that the perlite was not annealed.
[0131] Comparative Example 2
[0132] A self-cleaning membrane was prepared according to the method of Example 1, except that the perlite was not subjected to surface modification treatment.
[0133] Comparative Example 3
[0134] A self-cleaning membrane was prepared according to the method of Example 1, except that the perlite was not subjected to annealing treatment and surface modification treatment.
[0135] Comparative Example 4
[0136] A self-cleaning membrane was prepared according to the method of Example 1, except that the perlite in the raw material was not subjected to grinding, annealing and surface modification.
[0137] The contact angle and rolling angle of the self-cleaning films prepared in the above examples and comparative examples were tested using the standard ASTM F21-20. The test results are shown in Table 1.
[0138] The self-cleaning membrane prepared in Example 1 was subjected to mechanical property tests and waterproof performance tests, including
[0139] (1) Mechanical property test: The glass coated with the self-cleaning film was placed and fixed at 45° to the horizontal. Sand with different weights and particle sizes ranging from 0.5 mm to 1 mm was dropped from a height of 1.5 m to rub the coating. The contact angle before and after each friction test, as well as the mass change, were recorded. The graph of the contact angle versus friction intensity is shown in Figure 2. Figure 3 As shown, the data in part a represents the contact angle, and the data in part b represents the mass change. As the friction intensity increases, the contact angle rises briefly and then begins to decline, and then remains at around 123°. At the same time, the rolling angle remains between 2° and 7°, that is, the self-cleaning film in this application has excellent mechanical properties.
[0140] (2) Waterproof performance test: The glass coated with the self-cleaning film was placed in water with a depth of 10 cm and immersed for different lengths of time. The contact angle and rolling angle were recorded before and after each immersion test. The contact angle changes during the same immersion time were as follows: Figure 4 As shown, as the soaking time increases, the contact angle of the self-cleaning film decreases in a short period of time, and then begins to rise back to the original level. At the same time, during this process, the rolling angle remains at 2° to 5°, that is, the waterproof performance of the self-cleaning film in this application is good.
[0141] Table 1
[0142]
[0143]
[0144] From the above table we can see that:
[0145] (1) From Examples 1 and 9-10, it can be seen that the present application controls the temperature of the annealing treatment, removes the organic components in the perlite, increases the proportion of the lamellar structure in the perlite, and improves the surface modification effect. If the annealing temperature is low, the organic components may not be completely removed, resulting in a decrease in the hydrophobicity of the material; if the annealing temperature is high, the microstructure of the perlite material may be affected, thereby affecting the surface energy of the material.
[0146] (2) From Examples 1 and 11-12, it can be seen that the present application controls the quality of the surfactant, reduces the surface energy of the perlite material, and improves the hydrophobicity. If the quality is relatively low, the surface modification of the perlite may be incomplete, affecting the reduction of the surface energy and poor hydrophobicity; if the quality is relatively high, it may cause the surfactant to remain, thereby affecting the hydrophobicity of the self-cleaning film formed by the modified perlite.
[0147] (3) Compared with Comparative Examples 1-4, Example 1 shows that: In Example 1, the optical microscope photo of the untreated perlite in the raw material is as follows: Figure 5 As shown in the figure, it can be seen that the spatial structure of perlite is a hollow microsphere structure, and its particle size is about 500μm. The optical microscope photo of the ground perlite is shown in the figure below. Figure 6 As shown in Figure 1, the spatial structure of the perlite after grinding is irregular flake and block structure, and its particle size is about 40μm. The optical microscope photo of the perlite after annealing is shown in Figure 1. Figure 7 As shown, the spatial structure of perlite is a flake and block structure with similar geometric shapes. What is different from before annealing is that the proportion of flat flake structures has greatly increased. The fragments of these flake structures are arranged in parallel, vertical, or intersecting ways, and the particle size is about 40μm.
[0148] Through the above embodiments and comparative examples, the present application anneals and modifies the perlite surface, thereby reducing the surface energy of the perlite material and improving the hydrophobic performance of the self-cleaning film. The contact angle between the self-cleaning film and water reaches about 155°, and the rolling angle is below 5°; and after the perlite is annealed, the proportion of perlite flaky structure is increased, the surface roughness of the material and the gas-liquid contact surface are improved, and the surface energy of the material itself is reduced, and the surface modification ability of the perlite is improved. When water falls on the self-cleaning material layer of the present application, it can quickly pass through the surface of the self-cleaning material layer, and at the same time take away pollutants such as dust on the surface, so as to achieve the effect of self-cleaning of the component, and has the characteristics of good environmental tolerance and high mechanical strength.
[0149] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0150] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a self-cleaning membrane, characterized in that: The preparation method comprises: The annealed perlite is surface modified by using a surfactant to obtain modified perlite; According to the weight percentage, 50 to 85 parts of the modified perlite, 3 to 19 parts of acrylic resin and 12 to 36 parts of solvent are mixed, and then coated to obtain the self-cleaning film; The annealing treatment satisfies: the atmosphere of the annealing treatment is a protective atmosphere, the temperature of the annealing treatment is 300° C. to 550° C., and the time is 0.5 h to 1.5 h; The surfactant is silanol, and the mass of the surfactant is 5% to 9% of the mass of the perlite.
2. The preparation method according to claim 1, characterized in that The protective atmosphere includes at least one of an inert gas and nitrogen.
3. The preparation method according to claim 1, characterized in that: The particle size of the perlite is 10 μm to 50 μm.
4. The preparation method according to claim 1, characterized in that: The perlite is ground before the annealing process.
5. The preparation method according to claim 1, characterized in that: The perlite has a flaky structure and a block structure.
6. The preparation method according to claim 1, characterized in that: The surface modification method comprises: The annealed perlite is mixed with a surfactant to form a solution, and the solution is dried to obtain the modified perlite.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The acrylic resin includes at least one of isobutyl methacrylate / styrene resin, butyl acrylate resin, methacrylate resin, methyl methacrylate resin and methyl methacrylate / styrene resin.
8. The preparation method according to any one of claims 1 to 6, characterized in that: The solvent includes xylene.
9. A self-cleaning membrane, characterized in that: The self-cleaning film is prepared by the method for preparing a self-cleaning film according to any one of claims 1 to 8. The self-cleaning film comprises an acrylic resin substrate layer and modified perlite dispersed on the surface of the acrylic resin substrate layer.
10. The self-cleaning membrane according to claim 9, characterized in that The thickness of the self-cleaning film is 0.01 mm to 1 mm.
11. A photovoltaic module, characterized in that: The photovoltaic module comprises the self-cleaning film according to claim 9 or 10.
Citation Information
Patent Citations
Super-hydrophobic coating for photovoltaic module and preparation method of super-hydrophobic coating
CN116445050A