Preparation method of hollow spherical ammonium perchlorate

Ammonium perchlorate was prepared by recrystallization in oleic acid, which solved the problems of irregular morphology and high production cost of ammonium perchlorate, and obtained hollow spherical ammonium perchlorate with high sphericity and uniform particle size, which is suitable for Industrialized production and reduced waste disposal.

CN117285011BActive Publication Date: 2024-10-01JIANGSU MINGKONG AEROSPACE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311156235.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-08
Publication Date
2024-10-01
Estimated Expiration
2043-09-08

AI Technical Summary

Technical Problem

Existing methods for controlling the morphology of ammonium perchlorate have problems such as irregular morphology, high risk, and high production costs. In particular, the application prospects of spherical ammonium perchlorate in propellants have not been fully utilized.

Method used

Using oleic acid as an antisolvent, by recrystallizing the ammonium perchlorate solution in oleic acid and controlling the feeding rate, temperature and stirring conditions, hollow spherical ammonium perchlorate with high sphericity and uniform particle size is prepared.

Benefits of technology

This method achieves the preparation of ammonium perchlorate with high sphericity, uniform particle size and good dispersion, reduces production costs, avoids the use of surfactants, is suitable for industrial production, and can reuse solvents to reduce waste disposal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117285011B_ABST
    Figure CN117285011B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing hollow spherical ammonium perchlorate. Oleic acid is used as an anti-solvent, an ammonium perchlorate solution is added to the oleic acid anti-solvent, and the hollow spherical ammonium perchlorate is prepared by crystallization. The obtained hollow spherical ammonium perchlorate has a particle size of 10 to 50 microns, high sphericity and good dispersibility. The method of the invention has a simple preparation process, is easy to operate, and has low raw material price and low cost, and is very suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method, in particular to a preparation method of hollow spherical ammonium perchlorate. Background Art

[0002] Ammonium perchlorate has the advantages of high thermal stability, good chemical stability, low mechanical sensitivity and low price. It is a commonly used oxidant in solid propellants, accounting for 60% to 80% of the mass fraction of solid propellants. The morphology of ammonium perchlorate has a great influence on the performance of solid propellants, so the research on the morphology control of ammonium perchlorate has always attracted much attention.

[0003] There are usually two ways to control the morphology of ammonium perchlorate. One is the solid phase method, which involves mechanical ball milling, air flow crushing, etc. The solid phase method can change the morphology of ammonium perchlorate, but the resulting product is often irregular in morphology, and ammonium perchlorate is a strong oxidant, so the processes of ball milling and crushing are dangerous. The second is the liquid phase crystallization method, which involves cooling crystallization, evaporation crystallization, anti-solvent crystallization, etc. For example, Wang Yi (CN111410209A) added a crystal stabilizer to an aqueous solution of ammonium perchlorate, then injected it into a micro high-pressure atomizer, and then sprayed it into liquid nitrogen. After freeze drying, a mesh-like nano-scale ammonium perchlorate was crystallized. M. Kohga (Adv. Powder Tech. 21 (2010) 443–447) prepared hexahedral ammonium perchlorate by cooling crystallization of a saturated solution of ammonium perchlorate ethylene glycol. AA Vargeese (Crystal Growth Design, 8 (2008) 1060-1066) used water-soluble PVA as a surfactant to crystallize ammonium perchlorate to prepare wedge-shaped ammonium perchlorate. Wei Yanan (CN113620253A) added sodium dodecylbenzene sulfonate as a bulking agent, and vacuum distilled the ammonium perchlorate aqueous solution to obtain crystals, thereby preparing expanded ammonium perchlorate. Ma Zhenye (CN102718187A) first dissolved ammonium perchlorate in a mixed solvent of N, N-dimethylformamide / acetone to prepare a saturated solution, and then added it to the anti-solvent ethyl acetate to crystallize and obtain hollow cubic ammonium perchlorate.

[0004] Compared with ammonium perchlorate with other morphologies, spherical ammonium perchlorate has a higher accumulation coefficient, lower casting viscosity and higher load in propellants, and has broader application prospects in the field of propellants. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing hollow spherical ammonium perchlorate. The improved anti-solvent crystallization method is used to prepare the hollow spherical ammonium perchlorate product. The obtained ammonium perchlorate has high sphericity, uniform particle size and good dispersibility, and is more suitable for industrial production.

[0006] The technical solution of the present invention is: a method for preparing hollow spherical ammonium perchlorate, using oleic acid as an anti-solvent, adding an ammonium perchlorate solution into the oleic acid anti-solvent, crystallizing, and preparing hollow spherical ammonium perchlorate; the specific steps are as follows:

[0007] (1) At room temperature, dissolving ammonium perchlorate in a solvent to form an ammonium perchlorate solution of a certain concentration;

[0008] (2) adding the ammonium perchlorate solution to an oleic acid anti-solvent at a certain temperature at a certain feeding rate for recrystallization; after a period of time, separating, washing, and drying the product to obtain hollow spherical ammonium perchlorate.

[0009] In step (1), the solvent is one of N,N-dimethylformamide, dimethyl sulfoxide, and N-methylpyrrolidone.

[0010] In step (1), the certain concentration of ammonium perchlorate solution is 0.8 to 4.1 mol / L.

[0011] In step (2), the certain feed rate is 2 to 20 mL / min; the certain temperature is 15 to 50 °C; and the reaction time is 10 to 40 min.

[0012] In step (2), the volume ratio of the ammonium perchlorate solution to the oleic acid is controlled at 0.1 to 0.01, the recrystallization process is carried out under stirring at 500-800 rpm, the product is washed multiple times with ethyl acetate, and dried at 60°C.

[0013] The preparation principle of the invention is as follows: compared with the conventional ammonium perchlorate anti-solvents such as ethyl acetate and ether, the oleic acid anti-solvent has high viscosity, and the ammonium perchlorate solution is added to the high-viscosity oleic acid anti-solvent and is first dispersed into metastable spherical droplets under stirring, and then as the ions in the droplets diffuse outward, ammonium perchlorate crystals are formed on the surface of the spherical droplets, and finally the spherical hollow structure ammonium perchlorate is assembled.

[0014] The beneficial effects of the present invention are:

[0015] 1. Different from the traditional anti-solvent crystallization process, the method of the present invention will first form metastable spherical droplets of ammonium perchlorate wrapped by a high-viscosity oleic acid anti-solvent during the crystallization process, and then the surface of the droplet provides a crystallization template for the construction of spherical hollow structure ammonium perchlorate, and the spherical morphology is good.

[0016] 2. The raw materials used are simple, only industrial ammonium perchlorate and oleic acid are needed, and the production cost is low.

[0017] 3. No surfactant is introduced during production, which is environmentally friendly.

[0018] 4. The solvent and oleic acid after ammonium perchlorate crystallization can be separated and reused, reducing waste treatment processes and emissions.

[0019] 5. The preparation process and the required production equipment are simple and suitable for industrial production.

[0020] 6. The prepared ammonium perchlorate has high sphericity, a particle size of 10 to 50 microns, and good dispersibility.

[0021] 7. The raw material ammonium perchlorate has no restrictions on particle size, morphology, or crystal form.

[0022] 8. The present invention can be extended to the preparation of other spherical crystalline materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a scanning electron microscope image of the spherical hollow structure ammonium perchlorate obtained in Example 1;

[0024] Figure 2 This is a scanning electron microscope image of the spherical hollow structure ammonium perchlorate obtained in Example 2;

[0025] Figure 3 This is a scanning electron microscope image of the spherical hollow structure ammonium perchlorate obtained in Example 3;

[0026] Figure 4 This is the X-ray diffraction pattern of the spherical hollow structure ammonium perchlorate obtained in Example 1;

[0027] Figure 5 This is a scanning electron microscope image of the ammonium perchlorate obtained in Comparative Example 1;

[0028] Figure 6 This is a scanning electron microscope image of the ammonium perchlorate obtained in Comparative Example 2;

[0029] Figure 7 This is a scanning electron microscope image of the ammonium perchlorate obtained in Comparative Example 3. DETAILED DESCRIPTION

[0030] The technical solution of the present invention is further illustrated below in conjunction with embodiments and comparative examples, but they should not be construed as limitations on the technical solution, and all adaptive improvements based on these examples fall within the protection scope of the present invention.

[0031] Example 1: Take the following steps to prepare hollow spherical ammonium perchlorate

[0032] (1) At room temperature, dissolve ammonium perchlorate in N,N-dimethylformamide to form an ammonium perchlorate solution with a concentration of 0.8 mol / L;

[0033] (2) The ammonium perchlorate solution was added to an oleic acid anti-solvent at 15°C at a feeding rate of 2 mL / min for recrystallization; after 10 min, the product was separated, washed with ethyl acetate for multiple times, and dried at 60°C to obtain hollow spherical ammonium perchlorate; wherein the volume ratio of the ammonium perchlorate solution to oleic acid was controlled at 0.01, and the recrystallization process was carried out under stirring at 500 rpm.

[0034] Example 2: Take the following steps to prepare hollow spherical ammonium perchlorate

[0035] (1) At room temperature, ammonium perchlorate is dissolved in dimethyl sulfoxide to form an ammonium perchlorate solution with a concentration of 2.45 mol / L;

[0036] (2) adding the ammonium perchlorate solution to an oleic acid anti-solvent at 32.5° C. at a feeding rate of 11 mL / min for recrystallization; after 25 min, separating the product, washing it with ethyl acetate for multiple times, and drying it at 60° C. to obtain hollow spherical ammonium perchlorate; wherein the volume ratio of the ammonium perchlorate solution to oleic acid is controlled at 0.055, and the recrystallization process is carried out under stirring at 650 rpm.

[0037] Example 3: Take the following steps to prepare hollow spherical ammonium perchlorate

[0038] (1) At room temperature, dissolve ammonium perchlorate in N-methylpyrrolidone to form an ammonium perchlorate solution with a concentration of 4.1 mol / L;

[0039] (2) The ammonium perchlorate solution was added to an oleic acid anti-solvent at 50°C at a feeding rate of 20 mL / min for recrystallization; after 40 minutes, the product was separated, washed with ethyl acetate for multiple times, and dried at 60°C to obtain hollow spherical ammonium perchlorate; wherein the volume ratio of the ammonium perchlorate solution to oleic acid was controlled at 0.1, and the recrystallization process was carried out under stirring at 800 rpm.

[0040] Comparative Example 1: At room temperature, ammonium perchlorate was dissolved in N,N-dimethylformamide to form an ammonium perchlorate solution with a concentration of 4.5 mol / L; the ammonium perchlorate solution was added to an oleic acid anti-solvent at 30°C at a feeding rate of 14 mL / min for recrystallization; after 30 min, the product was separated, washed with ethyl acetate for multiple times, and dried at 60°C to obtain an ammonium perchlorate product; wherein the volume ratio of the ammonium perchlorate solution to oleic acid was controlled at 0.06, and the recrystallization process was carried out under stirring at 600 rpm.

[0041] Comparative Example 2: At room temperature, ammonium perchlorate was dissolved in dimethyl sulfoxide to form an ammonium perchlorate solution with a concentration of 2.2 mol / L; the ammonium perchlorate solution was added to an oleic acid anti-solvent at 55°C at a feeding rate of 16 mL / min for recrystallization; after 20 min, the product was separated, washed with ethyl acetate for multiple times, and dried at 60°C to obtain an ammonium perchlorate product; wherein the volume ratio of the ammonium perchlorate solution to oleic acid was controlled at 0.04, and the recrystallization process was carried out under stirring at 700 rpm.

[0042] Comparative Example 3: At room temperature, ammonium perchlorate was dissolved in N-methylpyrrolidone to form an ammonium perchlorate solution with a concentration of 0.6 mol / L; the ammonium perchlorate solution was added to an oleic acid anti-solvent at 40°C at a feeding rate of 20 mL / min for recrystallization; after 10 minutes, the product was separated, washed with ethyl acetate for multiple times, and dried at 60°C to obtain an ammonium perchlorate product; wherein the volume ratio of the ammonium perchlorate solution to oleic acid was controlled at 0.01, and the recrystallization process was carried out under stirring at 800 rpm.

[0043] Figure 1-Figure 3 The scanning electron microscope images of the spherical hollow structure ammonium perchlorate obtained in Examples 1-3 are respectively; Figure 4 This is the X-ray diffraction pattern of the spherical hollow structure ammonium perchlorate obtained in Example 1; Figure 5-Figure 7 They are scanning electron microscope pictures of the ammonium perchlorate products obtained in Comparative Examples 1-3 respectively; it can be seen from the figures that based on the principle and process of the present invention, spherical hollow structure ammonium perchlorate with high sphericity, uniform particle size and good dispersibility can be obtained.

Claims

1. A method for preparing hollow spherical ammonium perchlorate, characterized in that: Using oleic acid as an anti-solvent, adding an ammonium perchlorate solution into the oleic acid anti-solvent to crystallize and prepare hollow spherical ammonium perchlorate; the specific steps are as follows: (1) At room temperature, ammonium perchlorate is dissolved in a solvent to form an ammonium perchlorate solution of a certain concentration; the solvent is one of N,N-dimethylformamide, dimethyl sulfoxide, and N-methylpyrrolidone; the ammonium perchlorate solution of a certain concentration is 0.8 to 4.1 mol / L; (2) adding an ammonium perchlorate solution to an oleic acid anti-solvent at a certain temperature at a certain feeding rate for recrystallization; after a period of time, separating, washing, and drying the product to obtain hollow spherical ammonium perchlorate; the certain feeding rate is 2 to 20 mL / min; the certain temperature is 15 to 50° C.; the period of time is 10 to 40 min; the volume ratio of the ammonium perchlorate solution to the oleic acid is controlled at 0.1 to 0.01, and the recrystallization process is carried out under stirring at 500 to 800 rpm.

2. The method for preparing hollow spherical ammonium perchlorate according to claim 1, wherein: In step (2), the product is washed with ethyl acetate for multiple times and dried at 60°C.