A preparation process of highly water-resistant magnesium-phosphate cement-based material
By combining porous carbon materials that specifically adsorb phosphate ions with magnesium phosphate cement, the problem of insufficient water resistance of magnesium phosphate cement was solved, and the high water resistance and strength retention of magnesium phosphate cement were achieved.
Patent Information
- Application Number
- CN202311332500.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-10-16
AI Technical Summary
Magnesium phosphate cement has insufficient water resistance, and existing methods have failed to fundamentally improve the strength loss and efflorescence problems caused by the dissolution of phosphate ions.
Modified porous carbon materials are prepared by using porous carbon materials that specifically adsorb phosphate ions through pyrolysis carbonization and heat treatment under static air conditions. These modified porous carbon materials are then combined with reburned magnesium oxide, phosphate, borax, etc., to form a highly water-resistant magnesium phosphate cement-based material.
It effectively adsorbs phosphate ions, prevents their loss, restores the hydration reaction, significantly improves the water resistance of magnesium phosphate cement, and reduces strength loss and efflorescence.
Smart Images

Figure CN117285325B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of phosphate-magnesium cement-based materials, and in particular to a preparation process of a highly water-resistant phosphate-magnesium cement-based material. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Magnesium phosphate cement is a new type of special cement that sets and hardens quickly, has high early strength, and is compatible with ordinary Portland cement, so it is often used in rapid repair projects. However, the hydration product of magnesium phosphate cement, struvite (MgNH4PO4·6H2O), has weak water stability. After being eroded by water, the struvite is often dissolved into phosphate ions, ammonium ions, and magnesium ions, and migrates from the pores inside the magnesium phosphate cement to the outside, and recrystallizes on the surface of the magnesium phosphate cement to form struvite crystals again, causing the magnesium phosphate cement to lose strength seriously and cause large-scale "panning" phenomenon. Therefore, improving the water resistance of magnesium phosphate cement has always been a challenging task.
[0004] Due to the specificity of the composition of phosphate-magnesium cement, the amount of magnesium raw material used is often much greater than the amount of phosphorus raw material used. The remaining magnesium plays a supporting role inside the cement as a skeleton structure. The hydration product begins to nucleate and grow with magnesium as the skeleton, gradually cross-linking into a network structure, and finally forming a cement body. Since phosphorus is indispensable and its content is much lower than that of magnesium, reducing the dissolution of phosphorus is a fundamental measure to solve the water resistance of phosphate-magnesium cement. The main method at present is to add mineral admixtures and ultrafine powders to phosphate-magnesium cement. The purpose of this method is to allow finer mineral particles to be filled into the pores of cement, thereby reducing the entry of water from the external environment into the cement matrix. However, this method does not fundamentally improve the water resistance problem of phosphate-magnesium cement, and the prepared phosphate-magnesium cement still has the problem of insufficient water resistance. Summary of the invention
[0005] In view of the above problems, the present invention provides a preparation process of a highly water-resistant magnesium phosphate cement-based material. The present invention effectively improves the strength loss and efflorescence problems of magnesium phosphate cement caused by the dissolution of phosphate ions by using a porous carbon material that can specifically adsorb phosphate ions. To achieve the above objectives, the present invention discloses the following technical solutions.
[0006] A preparation process of a highly water-resistant magnesium-phosphate cement-based material comprises the following steps:
[0007] (1) The biomass carbon source is placed in a sealed heating furnace and subjected to pyrolysis and carbonization treatment under static air conditions. After completion, the carbonization product is cooled to room temperature, and the obtained carbonization product is mixed with a phosphorus source and ground into powder, and then the powder is placed in a sealed heating furnace and subjected to heat treatment under static air conditions. After completion, the product is cooled to room temperature, and then acid-washed, washed with water, and dried to obtain a modified porous carbon material.
[0008] (2) Compounding the modified porous carbon material with dead-burned magnesium oxide, ammonium dihydrogen phosphate or potassium dihydrogen phosphate, borax, fly ash, silica fume, fine aggregate, coarse aggregate and water to obtain a highly water-resistant magnesium phosphate cement-based material.
[0009] Furthermore, in step (1), the biomass carbon source includes but is not limited to at least one of chitosan, wheat straw, wood, rice straw, hemp stalks, etc.
[0010] In the present invention, the static air state means that during the heating process, the air in the heating environment is not circulated, or the outside air is not introduced. Instead, the atmospheric environment at the initial state of heating is used as the process environment until the pyrolysis carbonization treatment or heat treatment is completed, and the product obtained by the treatment continues to cool naturally to room temperature in this environment.
[0011] Furthermore, in step (1), the temperature of the pyrolysis carbonization treatment is 200 to 700° C., and the time is 2 to 8 hours.
[0012] Furthermore, in step (1), the mass ratio of the carbonized product to the phosphorus source is 1 to 3: 1. Preferably, the phosphorus source includes at least one of potassium dihydrogen phosphate, sodium acid pyrophosphate, sodium metaphosphate, manganese hypophosphite, metapyrophosphoric acid, and the like.
[0013] Furthermore, in step (1), the heat treatment temperature is 200-500° C. and the time is 2-8 hours. After the phosphorus source is introduced into the carbonized product, the heat treatment is performed again in a static air state to regulate the carbonized product to form positively charged oxygen vacancies, thereby forming a porous carbon material rich in such special oxygen vacancies.
[0014] Furthermore, in step (1), the pickling process is: placing the product in citric acid or acetic acid and stirring for 10 to 30 minutes, that is, completing the pickling process. Optionally, the mass fraction of the citric acid or acetic acid is 5 to 20%. Pickling helps to remove excess functional groups on the surface of the product, avoiding reaction with the cement matrix and reducing adsorption.
[0015] Furthermore, in step (1), the water washing process is: washing the product after acid washing with clean water until the washing liquid is neutral, thus completing the water washing process.
[0016] Furthermore, in step (1), the drying temperature is 30 to 70° C. and the drying time is 12 to 24 hours.
[0017] Furthermore, in step (2), the proportions of the raw materials are: 5 to 30 parts by weight of modified porous carbon material, 200 to 400 parts by weight of dead-burned magnesium oxide, 80 to 120 parts by weight of ammonium dihydrogen phosphate or potassium dihydrogen phosphate, 70 to 130 parts by weight of borax, 20 to 90 parts by weight of fly ash, 20 to 90 parts by weight of silica fume, 500 to 700 parts by weight of fine aggregate, 800 to 1600 parts by weight of coarse aggregate, and 150 to 300 parts by weight of water.
[0018] Optionally, the fineness of the ammonium dihydrogen phosphate or potassium dihydrogen phosphate, fly ash and silica fume is 100-300 mesh.
[0019] Compared with the prior art, the technical solution of the present invention has at least the following beneficial effects:
[0020] In view of the strength loss and alkali-fading problems caused by the dissolution of phosphate ions in the aforementioned magnesium-phosphate cement, the present invention prepares a porous carbon material that can specifically adsorb phosphate ions, and after combining it with magnesium-phosphate cement, the water resistance of magnesium-phosphate cement is fundamentally improved. This is because the porous carbon material prepared by the present invention using a special process has abundant oxygen vacancies and has obvious positive characteristics. It can specifically adsorb phosphate ions in cement paste, and this porous carbon material is chemically inert and can adsorb and release phosphate ions according to the concentration difference of phosphate ions in the internal environment of magnesium-phosphate cement. Thus: when magnesium-phosphate cement is eroded by water, the hydration product-struvite therein is dissolved into phosphate ions, etc., which will cause the concentration of phosphate ions inside magnesium-phosphate cement to increase. At this time, the excess phosphate ions will be adsorbed and stored in the porous carbon material without being lost to the outside of magnesium-phosphate cement. After restoring the normal environment without rainwater scouring, the ammonium ions and magnesium ions formed by the dissolution of struvite react with phosphate ions to form struvite crystals. As cement hydration proceeds, phosphate ions inside the magnesium-phosphate cement are gradually consumed. When the phosphate ion concentration is lower than the phosphate ion concentration inside the porous carbon material, the phosphate ions stored in the carbon material will be continuously released into the cement body to continue to participate in the hydration reaction, and new hydration products will be continuously generated until the hydration is complete. This effectively avoids the loss of low-content but indispensable phosphate ions due to dissolution, resulting in strength loss and alkali efflux in the magnesium-phosphate cement, thereby fundamentally improving the water resistance of the magnesium-phosphate cement.
[0021] In addition, to achieve the above-mentioned purpose, the present invention proposes a process for preparing a porous carbon material with abundant positively charged oxygen vacancies. First, the present invention performs pyrolysis carbonization treatment on a biomass carbon source under a static air state, so that while forming a carbonized product, a special site such as oxygen vacancies can also be introduced therein. Furthermore, the present invention also uses a phosphorus source to regulate the oxygen vacancies in the carbonized product. The presence of phosphorus is used to balance the charge, increase the vacancies, and increase the adsorption amount of phosphate ions. This is because the electronegativity of phosphorus is less than that of oxygen and carbon, so phosphorus is not as good as carbon and oxygen in attracting electrons, and phosphorus has a weaker adsorption capacity for electrons when forming oxygen vacancies. When oxygen atoms become superoxide radicals and electrons leave the matrix, they are less restricted, making it easier to create more oxygen vacancies on carbon materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. The embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein:
[0023] Figure 1 This is a rendering of the modified porous carbon material prepared in Example 1 of the present invention.
[0024] Figure 2 This is a diagram showing the effect of curing the test block prepared in Example 1 of the present invention in water.
[0025] Figure 3 This is a compressive strength test diagram of the test block prepared in Example 1 of the present invention.
[0026] Figure 4 This is a rendering of the effect of the modified porous carbon material prepared in Example 4 of the present invention. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0028] Unless otherwise defined, all professional and scientific terms used in the present invention have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions.
[0029] In addition, any method and material similar or equivalent to the described content can be applied to the method of the present invention. The technical solution of the present invention is further described in conjunction with the accompanying drawings and specific embodiments.
[0030] Example 1
[0031] A preparation process of a highly water-resistant magnesium-phosphate cement-based material comprises the following steps:
[0032] (1) Place chitosan in a tube furnace, seal the tube furnace, heat to 400° C. at a heating rate of 10° C. / min and keep the temperature for 5 hours in a static air state to perform pyrolysis and carbonization treatment on the chitosan. After completion, naturally cool to room temperature to obtain a carbonized product for standby use.
[0033] (2) The carbonized product and sodium metaphosphate are mixed in a mass ratio of 2:1 and ground into a 200 mesh powder. The powder is then placed in a tubular furnace. The tube furnace is sealed and heated to 400°C at a heating rate of 10°C / min in a static air state and kept warm for 3 hours for heat treatment. After completion, it is cooled to room temperature, and the obtained solid product is added to a 5% by mass citric acid solution and stirred for 30 minutes for acid washing. After completion, the solid product is separated by centrifugation and washed with clean water until the washing liquid is neutral. The solid product is then placed in an oven and dried at 70°C for 12 hours to obtain a modified porous carbon material (such as Figure 1 as shown), for backup.
[0034] (3) Take the following raw materials: 10 parts by weight of the modified porous carbon material prepared in this embodiment, 300 parts by weight of dead-burned magnesium oxide, 100 parts by weight of ammonium dihydrogen phosphate, 105 parts by weight of borax, 75 parts by weight of fly ash, 60 parts by weight of silica fume, 650 parts by weight of river sand fine aggregate, 1300 parts by weight of crushed stone coarse aggregate, and 260 parts by weight of water. Among them: the fineness of the ammonium dihydrogen phosphate, fly ash, and silica fume is 300 mesh. Add the solid components of the above raw materials into a mixer and dry mix for 2 minutes, then add the water and stir quickly for 3 minutes to obtain phosphate magnesium cement slurry.
[0035] 1. The modified porous carbon material prepared in this embodiment was subjected to synchrotron radiation X-ray absorption fine structure spectroscopy and Zeta potential test, and the results showed that the oxygen vacancy content was 2.57%, and the Zeta potential was 3.65 mV. It can be seen that the modified porous carbon material has abundant oxygen vacancies and exhibits obvious positive charge characteristics.
[0036] 2. Mass loss rate test: The magnesium phosphate cement slurry prepared in this example was poured into a mold with a size of 40×40×40 mm and demolded after six hours. Figure 2The specific calculation method of the mass loss rate is as follows: the mass of the test block before entering the water is recorded as A1, and after curing in water for 28 days, the test block is taken out of the water, and the water on the surface of the test block is wiped off, and the mass of the test block is measured as A2, and (A1-A2) / A1 is the mass loss rate.
[0037] 3. Strength loss rate test: The phosphate magnesium cement slurry prepared in this embodiment is poured into a mold with a size of 40×40×40 mm and demolded after six hours. Then it is cured in the air for 28 days to obtain a test block. The test block is prepared in the same way and placed in water for curing for 28 days after demolding. The specific calculation method of the strength loss rate is: the compressive strength of the test block obtained by curing in the air for 28 days is recorded as B1 (reference Figure 3 ), the compressive strength of the test block obtained by curing in water for 28 days is recorded as B2, and (B1-B2) / B1 is the strength loss.
[0038] The water resistance of the magnesium phosphate cement prepared by the present invention can be characterized by the mass loss rate and strength loss rate. The test results are: mass loss rate = 0.77%, strength loss rate = 20.04%.
[0039] Example 2
[0040] A preparation process of a highly water-resistant magnesium-phosphate cement-based material comprises the following steps:
[0041] (1) The crushed rice straw is placed in a tube furnace, and the tube furnace is sealed and heated to 700° C. at a heating rate of 10° C. / min in a static air state and kept at this temperature for 2 hours to perform pyrolysis and carbonization treatment on the rice straw. After completion, the rice straw is naturally cooled to room temperature to obtain a carbonized product, which is then used for later use.
[0042] (2) The carbonized product is mixed with potassium dihydrogen phosphate at a mass ratio of 1.5:1 and ground into a 200-mesh powder. The powder is then placed in a tubular furnace. The tube furnace is sealed and heated to 500°C at a heating rate of 10°C / min in a static air state and kept warm for 2 hours for heat treatment. After completion, it is cooled to room temperature, and the obtained solid product is added to a 10% by mass citric acid solution and stirred for 20 minutes for acid washing. After completion, the solid product is separated by centrifugation and washed with clean water until the washing liquid is neutral. The solid product is then placed in an oven and dried at 30°C for 24 hours to obtain a modified porous carbon material (such as Figure 4 as shown), for backup.
[0043] (3) Take the following raw materials: 30 parts by weight of the modified porous carbon material prepared in this embodiment, 400 parts by weight of dead-burned magnesium oxide, 120 parts by weight of potassium dihydrogen phosphate, 130 parts by weight of borax, 90 parts by weight of fly ash, 90 parts by weight of silica fume, 700 parts by weight of river sand fine aggregate, 1600 parts by weight of crushed stone coarse aggregate, and 300 parts by weight of water. Among them: the fineness of the potassium dihydrogen phosphate, fly ash, and silica fume is 100 mesh. The solid components of the above raw materials are first added to a mixer and dry mixed for 2 minutes, and then the water is added and quickly stirred for 3 minutes to obtain phosphate magnesium cement slurry.
[0044] 1. The modified porous carbon material prepared in this embodiment was tested by synchrotron radiation X-ray absorption fine structure spectrum. The results showed that the oxygen vacancy content was 2.68%, and the Zeta potential was 3.89 mV. It can be seen that the modified porous carbon material has abundant oxygen vacancies and exhibits obvious positive charge characteristics.
[0045] 2. The mass loss rate and strength loss rate of the magnesium-phosphate cement test block prepared in this embodiment were tested by the same method as in the above embodiment 1. The test results were: mass loss rate = 0.72%, strength loss rate = 17.54%.
[0046] Example 3
[0047] A preparation process of a highly water-resistant magnesium-phosphate cement-based material comprises the following steps:
[0048] (1) The crushed hemp stalks are placed in a tube furnace, and the tube furnace is sealed and heated to 200° C. at a heating rate of 10° C. / min in a static air state and kept at this temperature for 8 hours to perform pyrolysis and carbonization treatment on the hemp stalks. After completion, the hemp stalks are naturally cooled to room temperature to obtain a carbonized product, which is then used for later use.
[0049] (2) The carbonized product and sodium acid pyrophosphate are mixed in a mass ratio of 3:1 and ground into a 300-mesh powder. The powder is then placed in a tubular furnace, sealed in a static air state, heated to 200°C at a heating rate of 10°C / min and kept warm for 8 hours for heat treatment. After completion, it is cooled to room temperature, and the obtained solid product is added to a 20% by mass citric acid solution and stirred for 10 minutes for acid washing. After completion, the solid product is separated by centrifugation and washed with clean water until the washing liquid is neutral. The solid product is then placed in an oven and dried at 40°C for 18 hours to obtain a modified porous carbon material for later use.
[0050] (3) Take the following raw materials: 5 parts by weight of the modified porous carbon material prepared in this embodiment, 200 parts by weight of dead-burned magnesium oxide, 80 parts by weight of potassium dihydrogen phosphate, 70 parts by weight of borax, 20 parts by weight of fly ash, 20 parts by weight of silica fume, 500 parts by weight of river sand fine aggregate, 800 parts by weight of crushed stone coarse aggregate, and 150 parts by weight of water. Among them: the fineness of the potassium dihydrogen phosphate, fly ash, and silica fume is 200 mesh. Add the solid components of the above raw materials into a mixer and dry mix for 2 minutes, then add the water and stir quickly for 3 minutes to obtain phosphate magnesium cement slurry.
[0051] The modified porous carbon material prepared in this embodiment was tested by synchrotron radiation X-ray absorption fine structure spectroscopy, and the results showed that the oxygen vacancy content was 2.44%, and the Zeta potential was 3.51 mV. It can be seen that the modified porous carbon material has abundant oxygen vacancies and exhibits obvious positive charge characteristics.
[0052] 2. The mass loss rate and strength loss rate of the magnesium-phosphate cement test block prepared in this embodiment were tested by the same method as in the above embodiment 1. The test results were: mass loss rate = 0.86%, strength loss rate = 21.60%.
[0053] Example 4
[0054] A preparation process of a highly water-resistant magnesium-phosphate cement-based material, comprising the steps of: taking the following raw materials: 300 parts by weight of dead-burned magnesium oxide, 100 parts by weight of ammonium dihydrogen phosphate, 105 parts by weight of borax, 75 parts by weight of fly ash, 60 parts by weight of silica fume, 650 parts by weight of river sand fine aggregate, 1,300 parts by weight of crushed stone coarse aggregate, and 260 parts by weight of water. The fineness of the ammonium dihydrogen phosphate, fly ash, and silica fume is 300 mesh. The solid components in the above raw materials are first added to a mixer and dry mixed for 2 minutes, and then the water is added and quickly stirred for 3 minutes to obtain magnesium-phosphate cement slurry.
[0055] The mass loss rate and strength loss rate of the magnesium-phosphate cement test block prepared in this embodiment were tested by the same method as in the above embodiment 1. The test results were: mass loss rate = 1.79%, strength loss rate = 52.14%.
[0056] Example 5
[0057] A preparation process of a highly water-resistant magnesium-phosphate cement-based material comprises the following steps:
[0058] Take the following raw materials: 30 parts by weight of mineral particles (fly ash with a fineness of 300 mesh), 400 parts by weight of dead-burned magnesium oxide, 120 parts by weight of potassium dihydrogen phosphate, 130 parts by weight of borax, 90 parts by weight of fly ash, 90 parts by weight of silica fume, 700 parts by weight of river sand fine aggregate, 1600 parts by weight of crushed stone coarse aggregate, and 300 parts by weight of water. Among them, the fineness of the potassium dihydrogen phosphate, fly ash, and silica fume is 100 mesh. Add the solid components of the above raw materials into a mixer and dry mix for 2 minutes, then add the water and stir quickly for 3 minutes to obtain phosphorus magnesium cement slurry.
[0059] The mass loss rate and strength loss rate of the magnesium-phosphate cement test block prepared in this embodiment were tested by the same method as in the above embodiment 1. The test results were: mass loss rate = 1.64%, strength loss rate = 47.58%.
[0060] Example 6
[0061] A preparation process of a highly water-resistant magnesium-phosphate cement-based material comprises the following steps:
[0062] Take the following raw materials: 30 parts by weight of mineral particles (silica fume with a fineness of 400 mesh), 400 parts by weight of dead-burned magnesium oxide, 120 parts by weight of potassium dihydrogen phosphate, 130 parts by weight of borax, 90 parts by weight of fly ash, 90 parts by weight of silica fume, 700 parts by weight of river sand fine aggregate, 1600 parts by weight of crushed stone coarse aggregate, and 300 parts by weight of water. Among them, the fineness of the potassium dihydrogen phosphate, fly ash, and silica fume is 100 mesh. Add the solid components of the above raw materials into a mixer and dry mix for 2 minutes, then add the water and stir quickly for 3 minutes to obtain phosphate magnesium cement slurry.
[0063] The mass loss rate and strength loss rate of the magnesium-phosphate cement test block prepared in this embodiment were tested by the same method as in the above embodiment 1. The test results were: mass loss rate = 1.68%, strength loss rate = 46.27%.
[0064] Example 7
[0065] A preparation process of a highly water-resistant magnesium-phosphate cement-based material is the same as that of the above-mentioned embodiment 3, except that the modified porous carbon material of this embodiment is prepared by the following method:
[0066] (1) The crushed hemp stalks are placed in a tube furnace, and the tube furnace is sealed and heated to 200° C. at a heating rate of 10° C. / min in a static air state and kept at this temperature for 8 hours to perform pyrolysis and carbonization treatment on the hemp stalks. After completion, the hemp stalks are naturally cooled to room temperature to obtain a carbonized product, which is then used for later use.
[0067] (2) The carbonized product is added to a citric acid solution with a mass fraction of 20% and stirred for 10 minutes for acid washing. After completion, the solid product is separated by centrifugation and washed with clean water until the washing liquid is neutral. Then, the solid product is placed in an oven and dried at 40° C. for 12 hours to obtain a modified porous carbon material.
[0068] 1. The modified porous carbon material prepared in this embodiment was tested by synchrotron radiation X-ray absorption fine structure spectrum. The results showed that the oxygen vacancy content was 2.08%, and the Zeta potential was 2.95 mV. It can be seen that the oxygen vacancy content of the modified porous carbon material is low, and the positive charge characteristic is significantly weakened.
[0069] 2. The mass loss rate and strength loss rate of the magnesium-phosphate cement test block prepared in this embodiment were tested by the same method as in the above embodiment 1. The test results were: mass loss rate = 1.26%, strength loss rate = 36.5%.
[0070] Example 8
[0071] A preparation process of a highly water-resistant magnesium-phosphate cement-based material is the same as that of the above-mentioned embodiment 2, except that the modified porous carbon material of this embodiment is prepared by the following method:
[0072] (1) Pulverized rice straw and potassium dihydrogen phosphate are placed in a tube furnace at a mass ratio of 1.5:1, and the tube furnace is sealed and heated to 700°C at a heating rate of 10°C / min in a static air state and kept at this temperature for 2 hours to perform pyrolysis and carbonization treatment on the rice straw. After completion, the mixture is naturally cooled to room temperature to obtain a carbonized product, which is then used for later use.
[0073] (2) Grind the carbonized product into a 200-mesh powder, then add it to a 10% by mass citric acid solution and stir for 20 minutes for acid washing. After completion, centrifuge to separate the solid product, and wash it with clean water until the washing liquid is neutral. Then place the solid product in an oven and dry it at 30° C. for 24 hours to obtain a modified porous carbon material for later use.
[0074] 1. The modified porous carbon material prepared in this embodiment was tested by synchrotron radiation X-ray absorption fine structure spectrum. The results showed that the oxygen vacancy content was 2.17%, and the Zeta potential was 3.03 mV. It can be seen that the oxygen vacancy content of the modified porous carbon material is relatively low, and the positive charge characteristic is significantly weakened.
[0075] 2. The mass loss rate and strength loss rate of the magnesium-phosphate cement test block prepared in this embodiment were tested by the same method as in the above embodiment 1. The test results were: mass loss rate = 1.07%, strength loss rate = 25.33%.
[0076] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A preparation process of a highly water-resistant magnesium-phosphate cement-based material, characterized in that: The steps include: (1) placing a biomass carbon source in a sealed heating furnace and then performing pyrolysis carbonization treatment under static air conditions; after completion, cooling to room temperature, mixing the obtained carbonization product with a phosphorus source at a mass ratio of 1 to 3:1 and grinding the mixture into powder, and then placing the powder in a sealed heating furnace and then performing heat treatment under static air conditions; after completion, cooling to room temperature, acid-washing the obtained product, washing it with water, and drying it to obtain a modified porous carbon material; (2) 5-30 parts by weight of the modified porous carbon material, 200-400 parts by weight of dead-burned magnesium oxide, 80-120 parts by weight of ammonium dihydrogen phosphate or potassium dihydrogen phosphate, 70-130 parts by weight of borax, 20-90 parts by weight of fly ash, 20-90 parts by weight of silica fume, 500-700 parts by weight of fine aggregate, 800-1600 parts by weight of coarse aggregate, and 150-300 parts by weight of water are compounded to obtain a highly water-resistant magnesium phosphate cement-based material.
2. The preparation process of the highly water-resistant magnesium-phosphate cement-based material according to claim 1, characterized in that: In step (1), the biomass carbon source includes at least one of chitosan, wheat straw, wood, rice straw, and hemp stalks.
3. The preparation process of the highly water-resistant magnesium-phosphate cement-based material according to claim 1, characterized in that: In step (1), the temperature of the pyrolysis carbonization treatment is 200-700°C and the time is 2-8 hours.
4. The preparation process of the highly water-resistant magnesium-phosphate cement-based material according to claim 1, characterized in that: The phosphorus source includes at least one of potassium dihydrogen phosphate, sodium acid pyrophosphate, sodium metaphosphate, manganese hypophosphite, and metapyrophosphoric acid.
5. The preparation process of the highly water-resistant magnesium-phosphate cement-based material according to claim 1, characterized in that: In step (1), the heat treatment temperature is 200-500°C and the time is 2-8 hours.
6. The preparation process of the highly water-resistant magnesium-phosphate cement-based material according to claim 1, characterized in that: In step (1), the pickling process is: placing the product in citric acid or acetic acid and stirring for 10 to 30 minutes to complete the pickling process.
7. The preparation process of the highly water-resistant magnesium-phosphate cement-based material according to claim 6, characterized in that: The mass fraction of the citric acid or acetic acid is 5-20%.
8. The preparation process of the highly water-resistant magnesium-phosphate cement-based material according to claim 1, characterized in that: In step (1), the water washing process is: washing the product after acid washing with clean water until the washing liquid is neutral, thus completing the water washing process.
9. The preparation process of the highly water-resistant magnesium-phosphate cement-based material according to claim 1, characterized in that: In step (1), the drying temperature is 30-70°C and the drying time is 12-24 hours.
10. The process for preparing the highly water-resistant magnesium-phosphate cement-based material according to claim 9, characterized in that: The fineness of the ammonium dihydrogen phosphate or potassium dihydrogen phosphate, fly ash and silica fume is 100-300 mesh.