Application of benzoquinone small molecules as additives in the preparation of electrolytes

By using benzoquinone-based small molecules with redox reactivity as electrolyte additives in hybrid capacitors, the problems of dendrite growth and hydrogen evolution corrosion of the zinc anode are solved, and the electrochemical performance and cycle life of the hybrid capacitor are improved, making it suitable for commercialization application.

CN117292952BActive Publication Date: 2024-10-01SUN YAT SEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311213981.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-19
Publication Date
2024-10-01
Estimated Expiration
2043-09-19

AI Technical Summary

Technical Problem

The problems of dendrite growth, hydrogen evolution corrosion and surface passivation related to zinc anode hinder the development and widespread application of hybrid capacitors, resulting in shorter cycle life and lower safety of energy storage devices.

Method used

Introducing benzoquinone small molecules with redox reactivity as electrolyte additives, through hydrogen bonding and chemical adsorption of hydroxyl and aldehyde groups, inhibit dendrite growth, reshape the solvation shell structure of the zinc anode, and reduce hydrogen evolution corrosion , and promote the redox reaction of the electrolyte and improve the charge transfer efficiency.

Benefits of technology

It effectively improves the cycle life, safety and electrochemical performance of the hybrid capacitor, enhances the energy density and power density, reduces the cost, and is suitable for large-scale industrial production and commercial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117292952B_ABST
    Figure CN117292952B_ABST
Patent Text Reader

Abstract

The present invention discloses the application of benzoquinone small molecules as electrolyte additives, wherein the benzoquinone small molecules are benzoquinone small molecules containing hydroxyl groups and / or aldehyde groups, which can effectively improve the cycle life, safety and electrochemical performance of hybrid capacitors. The hybrid capacitor electrolyte of the present invention weakens the solvation interaction between zinc ions and water by adding benzoquinone small molecules, thereby alleviating the corrosion of the zinc negative electrode and promoting the potential for long-term circulation. At the same time, it can effectively improve the redox performance of the battery, increase the capacity and energy density of the battery, and ultimately improve the electrochemical performance of the hybrid capacitor. The present invention is simple, easy to operate, energy-saving and environmentally friendly, and plays an important role in the development and commercial application of hybrid capacitors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electrochemical technology, and specifically relates to the application of benzoquinone small molecules as additives in the preparation of electrolytes. Background Art

[0002] Lithium-ion batteries have dominated the global energy storage market for decades due to their superior energy density and power density. However, limited lithium metal resources, high costs and safety risks restrict their large-scale application. To meet the growing demand for renewable energy, rechargeable hybrid capacitors have attracted much attention. Hybrid capacitors are composed of "capacitor-type" positive electrode materials and "battery-type" negative electrode materials, combining two different electrochemical mechanisms to achieve a balance between high energy density and high power density. First, zinc metal is used as a battery-type negative electrode with high capacity (820mAh g -1 ,5854mAhL -1 ) and low redox potential (-0.76V vs. standard hydrogen electrode), and abundant reserves and green environmental protection. Secondly, the use of water-based electrolyte ensures fast ion transfer kinetics, intrinsic safety, low cost and almost zero pollution.

[0003] However, problems such as dendrite growth, hydrogen evolution corrosion, and surface passivation associated with the zinc negative electrode have hindered the development and widespread application of hybrid capacitors. These problems lead to a short cycle life and low safety of energy storage devices, so it is necessary to study the modification of hybrid capacitors. Domestic and foreign researchers have made a lot of efforts to improve the stability of zinc negative electrodes, such as constructing layered structures, constructing artificial protective layers, and preparing electrolytes. Among them, the introduction of electrolyte additives is a convenient and effective method to stabilize the zinc negative electrode. Adding a small amount of additives has been proven to effectively guide the uniform distribution and deposition of zinc ions, thereby inhibiting the formation of dendrites and improving the stability and coulombic efficiency of hybrid capacitors. Therefore, how to innovatively introduce a pollution-free, environmentally friendly, low-cost, and simple-process electrolyte additive is of great significance for the improvement of the electrochemical performance and commercial application of hybrid capacitors. Summary of the invention

[0004] In order to overcome the problems existing in the above-mentioned prior art, one of the purposes of the present invention is to provide the use of benzoquinone small molecules as additives in the preparation of electrolytes. The second purpose of the present invention is to provide a hybrid capacitor electrolyte. The third purpose of the present invention is to improve the electrochemical properties of aqueous electrolytes.

[0005] Redox-Enhanced Electrolyte is a special type of electrolyte used in electrochemical energy storage systems. It enhances the performance of the electrolyte by introducing redox reaction substances, thereby improving the energy density, power density and cycle life of energy storage devices. Traditional electrolytes are mainly composed of electrolyte salts dissolved in organic solvents, which are used to provide a medium for ion transmission. On the basis of traditional electrolytes, redox-enhanced electrolytes add substances with reversible electrochemical activity to provide additional "electrical energy-chemical energy" energy conversion, thereby improving the electrochemical performance of secondary batteries or supercapacitors. By introducing redox-enhanced additives and improving the structural composition and interface properties of the electrolyte, energy storage with higher energy density, power density and cycle life can be achieved to meet the needs of high-performance energy storage devices and promote the development and commercial application of electrochemical energy storage technology. Through multiple experiments, the inventors found that redox-reactive benzoquinone small molecules as electrolyte additives are the most effective way to improve the electrochemical performance of hybrid capacitors.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] The first aspect of the present invention provides the use of benzoquinone small molecules as additives in the preparation of electrolytes, wherein the benzoquinone small molecules are benzoquinone small molecules containing hydroxyl groups and / or aldehyde groups.

[0008] Preferably, the benzoquinone small molecules include rhodiolac acid, crotonic acid, halogenated hydroxybenzoquinone, dihydroxybenzoquinone or tetrahydroxybenzoquinone, and corresponding salts or derivatives; the halogenated hydroxybenzoquinone includes 2,5-dichloro-3,6-dihydroxy-p-benzoquinone and 2,5-dibromo-3,6-dihydroxy-p-benzoquinone.

[0009] The term "salt" refers to salts of the compounds of the present invention, prepared from the compounds having specific substituents discovered in the present invention and relatively non-toxic acids or bases. Electrochemically acceptable salts are preferred.

[0010] More preferably, the benzoquinone small molecules include rhodiolacid, sodium rhodiolacid, crotonic acid, sodium crotonate, 2,5-dichloro-3,6-dihydroxy-p-benzoquinone and 2,5-dibromo-3,6-dihydroxy-p-benzoquinone, 2,5-dihydroxy-p-benzoquinone, tetrahydroxybenzoquinone, tetrahydroxybenzoquinone disodium salt, and tetrahydroxybenzoquinone tetrasodium salt.

[0011] Further preferably, the electrolyte includes a hybrid capacitor electrolyte, a zinc ion battery electrolyte, a lithium ion battery electrolyte, a lithium sulfur battery electrolyte, a sodium ion battery electrolyte, a potassium ion battery electrolyte, a calcium ion battery electrolyte, and a magnesium ion battery electrolyte.

[0012] The second aspect of the present invention provides a hybrid capacitor electrolyte, wherein the hybrid capacitor electrolyte uses the benzoquinone small molecules described in the first aspect of the present invention as additives, and the benzoquinone small molecules are benzoquinone small molecules containing hydroxyl groups and / or aldehyde groups.

[0013] Preferably, the concentration of the benzoquinone small molecule in the hybrid capacitor electrolyte is 0.01-1000 mmol·L -1 More preferably 0.1-50mmol·L -1 ; More preferably 0.5-10mmol·L -1 .

[0014] Preferably, the operating current range of the hybrid capacitor electrolyte is 0.01-50 mA·cm -2 More preferably, 0.1-5 mA·cm -2 ; More preferably 1-3mA·cm -2 .

[0015] Preferably, the hybrid capacitor electrolyte is a zinc ion hybrid capacitor electrolyte.

[0016] Preferably, the zinc ion hybrid capacitor electrolyte includes a soluble zinc salt; the soluble zinc salt is one or more of zinc sulfate, zinc trifluoromethanesulfonate, zinc bistrifluoromethanesulfonate imide, zinc perchlorate, zinc sulfate, zinc chloride, zinc nitrate, zinc acetate, zinc fluoride, zinc hexafluoride, zinc tetrafluoroborate and zinc gluconate.

[0017] Preferably, the concentration of the soluble zinc salt is 0.1-10 mol·L -1 More preferably, 1-3 mol·L -1 .

[0018] Preferably, the zinc ion hybrid capacitor electrolyte also includes a solute compound; the solute compound is one or more of sodium chloride, potassium chloride, magnesium chloride, sodium sulfate, potassium sulfate, magnesium sulfate, sodium hydroxide, potassium hydroxide, sodium trifluoromethanesulfonate, potassium trifluoromethanesulfonate, magnesium trifluoromethanesulfonate, hydrochloric acid, and sulfuric acid.

[0019] Preferably, the negative electrode of the battery suitable for the zinc ion hybrid capacitor electrolyte is metallic zinc or metallic zinc-modified metal;

[0020] Preferably, the zinc ion hybrid capacitor electrolyte is suitable for a battery positive electrode of at least one of manganese-based oxides, Prussian blue derivatives, vanadium-based materials, polyanion compounds, Chevrel phase compounds, activated carbon, and organic positive electrode materials.

[0021] More preferably, the manganese-based oxide comprises at least one of MnO2, Mn2O3, Mn3O4 and MnO; the Prussian blue derivative comprises KCu[Fe 3+ (CN)6], CuHCF and ZnHCF; the vanadium-based material includes at least one of NaV3O8, V2O5, VO2 and VS2; the polyanion compound includes at least one of Na3V2(PO4)3, VOPO4·xH2O and Li3V2(PO4)3; the Chevrel phase compound includes at least one of Mo6S8, Mo6Se8 and Mo6Te8; the activated carbon includes pure activated carbon and a mixture; the organic positive electrode material includes at least one of p-chloranil, calix quinone and TAPQ; further preferably, the MnO2 includes at least one of 2×2 tunnel-shaped α-MnO2, 1×1 tunnel-shaped β-MnO2 and layered δ-MnO2.

[0022] The third aspect of the present invention provides a hybrid capacitor and improves its electrochemical performance, comprising the electrolyte described in the second aspect of the present invention.

[0023] The beneficial effects of the present invention are:

[0024] The present invention discloses the application of benzoquinone small molecules as electrolyte additives. The use of benzoquinone small molecules containing hydroxyl groups and / or aldehyde groups can effectively improve the cycle life, safety and electrochemical performance of hybrid capacitors.

[0025] Specifically, compared with the prior art, the present invention has the following advantages:

[0026] 1. In the benzoquinone electrolyte additive of the present invention, the benzoquinone small molecules can be tightly adsorbed on the electrode / electrolyte interface, and form an adsorption layer through the hydrogen bonding between molecules, thereby preventing water, SO4 2- Direct contact with the Zn surface can inhibit the occurrence of side reactions and reduce dendrite growth. At the same time, the hydroxyl and aldehyde groups of benzoquinone small molecules have stronger chemical adsorption capacity for Zn. The introduction of chelating groups helps to reshape [Zn(H2O)6] 2+ The solvation shell structure weakens the electrochemical activity of water molecules, thereby achieving the purpose of desolvation, reducing hydrogen evolution corrosion, and protecting the zinc negative electrode. In addition, the introduction of hydroxyl and aldehyde functional groups promotes the redox reaction of the electrolyte. During the "charge-discharge" process, the mutual conversion of hydroxyl and aldehyde groups is utilized to enhance the charge transfer between "electrode-electrolyte", thereby providing additional capacity for the battery and improving the energy density of the hybrid capacitor.

[0027] 2. The hybrid capacitor electrolyte of the present invention weakens the solvation interaction between zinc ions and water by adding benzoquinone small molecules, thereby alleviating the corrosion of the zinc negative electrode and promoting the potential of long-term circulation; on this basis, the Zn-containing 2+ The electrolyte undergoes hydrolysis to produce H + The external electric field promotes the reversible transformation between "benzoquinone-phenol", thereby effectively improving the redox performance of the battery, increasing the capacity and energy density of the battery, and ultimately improving the electrochemical performance of the hybrid capacitor. The present invention is simple, easy to operate, energy-saving and environmentally friendly, and plays an important role in the development and commercial application of hybrid capacitors.

[0028] 3. The method of improving the stability of the zinc negative electrode by using benzoquinone small molecules containing active groups such as hydroxyl and aldehyde groups as electrolyte additives is simple, easy to operate, low cost, energy-saving and environmentally friendly. While effectively improving the cycle life of hybrid capacitors, combined with high-capacity positive electrode materials, it will help improve the actual energy density, cycle life and safety of energy storage devices, and is suitable for large-scale industrial production and commercial applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Photos of the additive aqueous solution and the redox-enhanced electrolyte prepared in Example 1, Example 2, Example 3, Example 4, Example 5, and Comparative Example 1;

[0030] Figure 2 The UV spectra and color changes of the redox enhanced electrolyte prepared in Example 1 at different voltages;

[0031] Figure 3 The aqueous zinc ion symmetric battery prepared in Example 1, Example 2, Example 3, Example 4, Example 5 and Comparative Example 1 was subjected to a temperature of 25° C. and a current density of 2 mA·cm -2 and 1mAh·cm -2 Time voltage curve under the conditions;

[0032] Figure 4 Cyclic voltammetry curves of the zinc ion hybrid capacitors prepared in Comparative Example 1 and Example 1;

[0033] Figure 5 The electrochemical impedance curves of aqueous zinc ion symmetrical batteries prepared in Example 1, Example 2, Example 3, Example 4, Example 5, and Comparative Example 1 are shown;

[0034] Figure 6 The electrochemical impedance curves of aqueous zinc ion symmetric batteries prepared in another embodiment 1, embodiment 2, embodiment 3, embodiment 4, embodiment 5, and comparative example 1 are shown;

[0035] Figure 7 Schematic diagram of the "electrode-electrolyte" interface reaction in the traditional electrolyte prepared in Comparative Example 1;

[0036] Figure 8 Schematic diagram of the redox enhanced “electrode-electrolyte” interface reaction prepared in Example 1. DETAILED DESCRIPTION

[0037] The present invention is further described in detail below through specific examples. The raw materials used in the following examples, unless otherwise specified, can be obtained from conventional commercial sources or prepared and separated by simple synthesis; the processes used, unless otherwise specified, are conventional processes in the art.

[0038] The benzoquinone small molecules described in the following examples are representative electrolyte additives. The specific Chinese and English names and English abbreviations, chemical structural formulas, molecular weights, suppliers and CAS numbers are shown in Table 1:

[0039] Table 1 Chinese and English names and English abbreviations, chemical structure, molecular weight, supplier and CAS number of representative electrolyte additives among benzoquinone organic small molecules

[0040]

[0041] Example 1 Application of Sodium Rose Bengalate as Electrolyte Additive in Hybrid Capacitors

[0042] At room temperature, 28753.00 mg of zinc sulfate heptahydrate was completely dissolved in 50 mL of deionized water, and then 10.70 mg of sodium rhodendronate (RZA, 1 mmol·L -1 ), and after being uniformly dissolved, it is used as an electrolyte for standby use. Activated carbon is used as the positive electrode, zinc foil is used as the negative electrode sheet, and glass fiber is used as the separator to assemble an aqueous zinc ion button-type CR2032 symmetrical battery. Among them, the preparation of the positive electrode and the negative electrode, the assembly of the button-type CR2032 symmetrical battery, and the assembly of the aqueous hybrid capacitor are specifically performed as follows:

[0043] (1) Preparation process of activated carbon positive electrode sheet: 800 mg activated carbon, 100 mg conductive carbon black, and 100 mg PVB were weighed in a mass ratio of 8:1:1, and then 5 μL of anhydrous ethanol was added to stir the mixture in an agate mortar. The mixture was ground for 10 minutes until a uniform slurry was formed. The mixture was then evenly coated on the surface of a stainless steel sheet using an applicator, dried in a vacuum drying oven at 60°C for 12 hours, and then taken out and cut into positive electrode sheets with a diameter of 12 mm.

[0044] (2) Preparation process of glass fiber diaphragm: Cut the uncontaminated glass fiber diaphragm into sheets with a diameter of 16 mm.

[0045] (3) Preparation process of negative electrode sheet: Use sandpaper to polish the surface of zinc foil, then cut it into negative electrode sheets with a diameter of 12 mm, add anhydrous ethanol for ultrasonic cleaning, put it in an oven for drying, and take it out for use.

[0046] (4) Assembly process of button-type CR2032 symmetrical battery and full battery: First, place the zinc sheet on the negative electrode shell side, then place the separator, drip the electrolyte to wet the separator, then place the zinc sheet (symmetrical battery) or positive electrode sheet (full battery), gasket, washer and positive electrode shell in turn, then place it in a static press for static pressure sealing, and place the assembled battery in a vacuum drying oven (25°C) for 4 hours for standby use. After that, the assembled symmetrical battery and AC / / Zn zinc ion hybrid capacitor were used for cycle performance testing.

[0047] The redox-enhanced electrolyte contains RZA additives such as Figure 1 The color of the RZA aqueous solution is orange-yellow, and the color changes after mixing with the zinc sulfate aqueous solution, which shows that RZA interacts with the ions in the electrolyte.

[0048] The prepared redox-enhanced electrolyte was tested by UV-visible absorption spectroscopy. Figure 2 As shown, the RZA additive has absorption peaks in the two ranges of 300-400nm and 400-550nm. The external electric field causes the structural transformation of the RZA additive, causing the absorption peak intensity in the 400-550nm band to weaken. The redox enhanced electrolyte shows obvious color changes under the action of the electric field.

[0049] The test results of the symmetrical battery are as follows Figure 3 As shown, the aqueous zinc ion symmetric battery at 25℃ and 2mA·cm -2 , 1mAh·cm -2 Under these conditions, the cycle life exceeds 400 h and the polarization voltage is 130 mV, showing a large polarization voltage, which is beneficial to reducing the nucleation barrier, refining the grains, and ensuring the uniform distribution of current in space, which is beneficial to uniform nucleation and promoting high-power energy storage.

[0050] Example 1 also conducted experiments with different concentrations of RZA additive as an electrolyte additive. The CV test results of the AC / / Zn zinc ion hybrid capacitor are shown in Figure 4 As shown in the figure, the low concentration, medium concentration, and high concentration correspond to the concentrations of RZA additives of 0.1, 0.5, and 1.0 mmol L -1 Although there is no obvious prominent peak in the CV curve, the integral area of ​​the curve increases with the increase of the concentration of the additive RZA, indicating that there is a continuous redox reaction in the electrolyte, which makes the energy storage device have additional capacity contribution.

[0051] Electrochemical impedance spectroscopy (EIS) sample preparation process: Use the above-prepared solution as the electrolyte to assemble a symmetrical battery, and use an electrochemical workstation to test its EIS value. The EIS test results of the aqueous zinc ion symmetrical battery are as follows: Figure 5 , 6 As shown, the EIS curves show a relatively small electrochemical impedance, that is, a relatively fast charge transfer and ion transfer rate.

[0052] It is mentioned in the literature [A reassessment of rhodizonic acid as a qualitative reagent] and [The structure of aqueous rhodizonic acid] that rhodizonic acid ion will undergo self-oxidation and ring contraction in aqueous solution to form sodium crotonate ion. It can be considered that the application of sodium crotonate as an electrolyte additive in hybrid capacitors is similar to that of sodium rhodizonic acid.

[0053] Example 2 Application of chloranilic acid as electrolyte additive in hybrid capacitors

[0054] At room temperature, 28753.00 mg of zinc sulfate heptahydrate was completely dissolved in 50 mL of deionized water, and then 10.45 mg of chloranilic acid (CHA, 1 mmol·L -1 ), and after being uniformly dissolved, it is used as an electrolyte for standby use. An aqueous zinc ion button-type CR2032 symmetrical battery is assembled using activated carbon as the positive electrode, zinc foil as the negative electrode sheet, and glass fiber as the separator. Among them, the preparation of the positive electrode and the negative electrode, the assembly of the button-type CR2032 symmetrical battery, and the EIS sample preparation test are all the same as those in Example 1.

[0055] Redox-enhanced electrolytes contain CHA additives such as Figure 1 The color of CHA aqueous solution is light pink, and the color changes after mixing with zinc sulfate aqueous solution, which indicates that CHA interacts with ions in the electrolyte.

[0056] The test results of the symmetrical battery are as follows Figure 3 As shown, the aqueous zinc ion symmetric battery at 25℃ and 2mA·cm -2 , 1mAh·cm -2 Under the same conditions, the cycle life exceeds 250h and the polarization voltage is 60mV, showing a small polarization voltage. However, the EIS test results of aqueous zinc ion symmetric batteries are as follows Figure 5 , 6 As shown, the EIS curve shows a large electrochemical impedance, which is caused by the charge transfer and ion transfer at the “electrode-electrolyte” interface.

[0057] Example 3 Application of 2,5-dihydroxy-1,4-benzquinol as electrolyte additive in hybrid capacitors

[0058] At room temperature, 28753.00 mg of zinc sulfate heptahydrate was completely dissolved in 50 mL of deionized water, and then 7.00 mg of 2,5-dihydroxy-1,4-benzquinone (HBQ, 1 mmol·L -1 ), and after being uniformly dissolved, it is used as an electrolyte for standby use. An aqueous zinc ion button-type CR2032 symmetrical battery is assembled using activated carbon as the positive electrode, zinc foil as the negative electrode sheet, and glass fiber as the separator. Among them, the preparation of the positive electrode and the negative electrode, the assembly of the button-type CR2032 symmetrical battery, and the EIS sample preparation test are all the same as those in Example 1.

[0059] The redox-enhanced electrolyte contains HBQ additives such as Figure 1 The color of the HBQ aqueous solution is orange-red, and the color changes after mixing with the zinc sulfate aqueous solution, which indicates that HBQ interacts with the ions in the electrolyte.

[0060] The test results of the symmetrical battery are as follows Figure 3 As shown, the aqueous zinc ion symmetric battery at 25℃ and 2mA·cm -2 , 1mAh·cm -2 Under the same conditions, the cycle life is 146h and the polarization voltage is 65mV, showing a small polarization voltage. However, the EIS test results of the aqueous zinc ion symmetric battery are as follows Figure 5 , 6 As shown, the EIS curve shows a large electrochemical impedance, that is, the charge transfer and ion transfer rates in the electrolyte are slow.

[0061] Example 4 Application of disodium tetrahydroxybenzoquinone as an electrolyte additive in hybrid capacitors

[0062] At room temperature, 28753.00 mg of zinc sulfate heptahydrate was completely dissolved in 50 mL of deionized water, and then 10.80 mg of tetrahydroxybenzoquinone disodium salt (TQ, 1 mmol·L -1 ), and after being uniformly dissolved, it is used as an electrolyte for standby use. An aqueous zinc ion button-type CR2032 symmetrical battery is assembled using activated carbon as the positive electrode, zinc foil as the negative electrode sheet, and glass fiber as the separator. Among them, the preparation of the positive electrode and the negative electrode, the assembly of the button-type CR2032 symmetrical battery, and the EIS sample preparation test are all the same as those in Example 1.

[0063] Redox-enhanced electrolytes contain TQ additives such as Figure 1 The color of TQ aqueous solution is orange-yellow, and there is a certain color change after mixing with zinc sulfate aqueous solution, which shows that TQ interacts with ions in the electrolyte.

[0064] The test results of the symmetrical battery are as follows Figure 3 As shown, the aqueous zinc ion symmetric battery at 25℃ and 2mA·cm -2 , 1mAh·cm -2 Under the same conditions, the cycle life is 105h and the polarization voltage is 47mV, showing a small polarization voltage. However, the EIS test results of aqueous zinc ion symmetric batteries are as follows Figure 5 , 6 As shown, the EIS curve shows a relatively large electrochemical impedance, which is caused by the charge transfer and ion transfer at the “electrode-electrolyte” interface.

[0065] Example 5 Application of tetrahydroxy-1,4-benzoquinone hydrate as electrolyte additive in hybrid capacitors

[0066] At room temperature, 28753.00 mg of zinc sulfate heptahydrate was completely dissolved in 50 mL of deionized water, and then 9.51 mg of tetrahydroxy-1,4-benzoquinone hydrate (THQ, 1 mmol·L -1 ), and after being uniformly dissolved, it is used as an electrolyte for standby use. Zinc foil is used as an electrode sheet and glass fiber is used as a separator to assemble an aqueous zinc ion button-type CR2032 symmetrical battery. Among them, the preparation of the positive electrode and the negative electrode, the assembly of the button-type CR2032 symmetrical battery, and the EIS sample preparation test are all the same as those in Example 1.

[0067] The redox-enhanced electrolyte contains THQ additives such as Figure 1 The color of THQ aqueous solution is light brown. After mixing with zinc sulfate aqueous solution, the color is close to colorless and there are insoluble substances, which shows that THQ interacts with ions in the electrolyte.

[0068] The test results of the symmetrical battery are as follows Figure 3 As shown, the aqueous zinc ion symmetric battery at 25℃ and 2mA·cm -2 , 1mAh·cm -2 Under the same conditions, the cycle life is 71h and the polarization voltage is 47mV, showing a small polarization voltage. The EIS test results of the aqueous zinc ion symmetric battery are as follows Figure 5 , 6 As shown in Figure 2, the EIS curve shows a relatively small electrochemical impedance, which is beneficial to charge transfer and ion transfer. However, compared with RZA, THQ does not significantly improve the cycle life of aqueous zinc ion symmetric batteries.

[0069] Comparative Example 1 Composition and electrochemical performance test of conventional water-based hybrid capacitors

[0070] At room temperature, 28753.00 mg of zinc sulfate heptahydrate was completely dissolved in 50 mL of deionized water and was evenly dissolved for standby use. Zinc foil was used as the positive and negative electrodes and glass fiber was used as the diaphragm to assemble an aqueous zinc ion symmetrical battery. The preparation of the positive and negative electrodes, the assembly of the button-type CR2032 symmetrical battery, and the CV and EIS sample preparation tests were the same as those in Example 1.

[0071] The conventional electrolyte is prepared from aqueous zinc sulfate solution, such as Figure 1 The traditional electrolyte is transparent and does not change color under the action of the electric field.

[0072] The test results of the symmetrical battery are as follows Figure 3 As shown, the aqueous zinc ion symmetric battery at 25℃ and 2mA·cm -2 , 1mAh·cm -2 Under these conditions, the cycle life is only 59h and the polarization voltage is 52mV.

[0073] The cyclic voltammetry test results of AC / / Zn zinc ion hybrid capacitor are as follows Figure 4 As shown, the CV curve is quasi-rectangular, which is a typical feature of hybrid ion capacitors, but there is no additional capacity contribution.

[0074] The EIS test results of aqueous zinc ion symmetric battery are as follows Figure 5 , 6 As shown, the EIS curve shows a relatively small electrochemical impedance and weak ion conduction at the “electrode-electrolyte” interface.

[0075] In summary, adding soluble benzoquinone small molecules or salt substances to the aqueous electrolyte can effectively weaken the Zn 2+ and the solvation between water molecules, such as Figure 7 , 8 As shown, thus guiding Zn 2+ Uniform nucleation promotes uniform deposition / stripping process. This type of electrolyte additive improves the stability of the metal electrode, thereby effectively alleviating side reactions such as dendrite growth, surface passivation, and hydrogen evolution corrosion, thereby protecting the zinc negative electrode and improving the stability of the hybrid capacitor. At the same time, this type of electrolyte additive is represented by RZA, which has excellent redox properties through the mutual conversion between hydroxyl and aldehyde groups, promotes charge transfer at the "electrode-electrolyte" interface, and provides additional "electrical energy-chemical energy" energy conversion, which can effectively improve the specific capacity of the hybrid capacitor and increase the energy density of the energy storage device. In addition, the redox behavior of the electrolyte comes from the reversible "benzoquinone-phenol" conversion, and the H generated by the hydrolysis of ZnSO4 + Provided for benzoquinone reduction, OH -The method described in the present invention is simple in process and low in cost, and has great significance for improving the stability of hybrid capacitors and promoting their industrialization process.

[0076] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.

Claims

1. A hybrid capacitor, characterized in that: The electrolyte of the hybrid capacitor is a zinc ion hybrid capacitor electrolyte; the electrolyte of the hybrid capacitor uses benzoquinone small molecules as additives, and the benzoquinone small molecules are benzoquinone small molecules containing hydroxyl groups; the negative electrode of the hybrid capacitor is metal zinc or metal zinc modified metal.

2. The hybrid capacitor according to claim 1, characterized in that: The benzoquinone small molecules include rose palmitic acid, halogenated hydroxybenzoquinone, dihydroxybenzoquinone, tetrahydroxybenzoquinone, and corresponding salts or derivatives.

3. The hybrid capacitor according to claim 1, characterized in that: The concentration of the benzoquinone small molecule in the hybrid capacitor electrolyte is 0.01-1000 mmol·L -1 .

4. The hybrid capacitor according to claim 1, characterized in that: The zinc ion hybrid capacitor electrolyte includes a soluble zinc salt; the soluble zinc salt is one or more of zinc sulfate, zinc trifluoromethanesulfonate, zinc bistrifluoromethanesulfonate imide, zinc perchlorate, zinc sulfate, zinc chloride, zinc nitrate, zinc acetate, zinc fluoride, zinc hexafluoride, zinc tetrafluoroborate and zinc gluconate.

5. The hybrid capacitor according to claim 4, characterized in that: The concentration of the soluble zinc salt is 0.1-10 mol·L -1 .

6. The hybrid capacitor according to claim 1, characterized in that: The positive electrode of the hybrid capacitor is at least one of manganese-based oxides, Prussian blue derivatives, vanadium-based materials, polyanion compounds, Chevrel phase compounds, activated carbon, and organic positive electrode materials.