A packaging solder sheet and a method for preparing the same
Through the combination of alloy solder powder and micron-scale metal particles, the packaging solder sheet is directly molded, which solves the problem that existing welding materials cannot meet the low-temperature interconnection and high melting point service, and achieves efficient and reliable welding effects, which is suitable for large-scale production.
Patent Information
- Application Number
- CN202311284257.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-09-28
AI Technical Summary
The existing welding materials cannot meet the requirements of simple composition and process, strong reliability, can be produced on a large scale, and cannot be used for low-temperature interconnection and high melting point service in a short period of time.
The combination of alloy solder powder and micron-scale metal particles is used to form a packaging solder sheet with metal particles directly molded to achieve low-temperature welding and high-temperature service without the need for additives or adhesives, which is simple to operate and low-cost.
It realizes high melting point welding materials that are rapidly formed at low temperatures, improves the stability and reliability of welding, is suitable for large-scale production, and has excellent comprehensive mechanical properties.
Smart Images

Figure CN117300434B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of soldering sheets, and in particular to a packaging soldering sheet and a preparation method thereof. Background Art
[0002] With the rapid development of the electronics industry, the electronics industry is constantly moving towards miniaturization, high integration and high performance. Along with this comes the ever-increasing device power density, which causes the devices to be subjected to extremely high current density and great heat release, thus requiring the interconnection solder joints in electronic devices to withstand an increase in operating temperature. According to the requirements of traditional soft soldering interconnection, the melting point of the solder must be higher than the service temperature of the solder joint. The higher the service temperature, the higher the melting point of the solder needs to be selected, which means that the welding temperature needs to be increased. However, too high a welding temperature will not only damage the electronic devices, but also easily lead to unreliable connections.
[0003] Compared with traditional Si power devices, the third generation semiconductor high power devices represented by SiC and GaN have excellent performance such as large bandgap, high saturated electron drift rate, large critical breakdown strength, and high thermal conductivity. The service temperature of the third generation semiconductor is above 300°C, and the power density supported is much higher than that of the first generation Si semiconductor. This will inevitably lead to its rapid development and widespread application. It will also become the mainstream of semiconductor power devices. However, this poses new challenges to microelectronic packaging technology and interconnection materials. Developing interconnection materials that can stably serve in high melting point environments is one of the key issues in the current electronic packaging field.
[0004] At present, the main methods that can be used to solve the problem of high melting point service of electronic interconnection are high melting point solder, nano metal paste sintering and transient liquid phase diffusion soldering (TLP) technology. Among them, high melting point solders include gold-based alloy solders, zinc-based solders and high lead solders. Among gold-based solders, there are AuSn20 with a melting point of 280°C, AuGe12 with a melting point of 356°C and AuSi3 with a melting point of 363°C, but they contain a large amount of precious metals, which makes the cost extremely high and cannot be widely used. Some zinc-based solders can also be used for high melting point connections, such as ZnAl6 alloy with a melting point of 380°C, but they have the disadvantages of being easily oxidized and corroded. At present, the most widely used is still the environmentally unfriendly high lead solder, but with the increasingly stringent environmental regulations, it is imperative to find a substitute for high lead solder. As for nano metal paste, although it is used in the connection of some devices, the porosity inside the weld is high, the required welding time is long, and it often requires a more appropriate pressure, and the price is also relatively high. Although TLP technology can obtain high melting point metal compound (IMC) at a lower brazing temperature, the IMC formation speed is too slow to be mass-produced. Due to the above reasons, existing packaging materials and technologies can no longer fully meet the performance and reliability packaging requirements of power devices. Therefore, in order to meet the performance requirements of power devices, it is a general trend to develop a welding material that can perform low-temperature interconnection in a short time and has a high melting point.
[0005] Chinese invention patent CN104625466B discloses a bismuth-based / copper particle composite solder that can quickly form high melting point solder joints at low temperatures. The composite solder adds bismuth-based solder powder and copper particles to the flux paste for mixing to form a mixed solder paste. The solder paste can more easily form a high melting point welding joint during welding compared to ordinary solder. However, since the composite solder is in a paste form, the mixed solder paste can only be applied to the pad in the form of coating or spraying, which easily causes uneven coating, and the amount of solder is difficult to keep consistent, and it is impossible to fully adapt to the solderable area of the pad. At the same time, since the solder paste contains more flux, the flux is easy to volatilize during reflow, causing a large area of gaps, thereby reducing the reliability of the solder joints.
[0006] Chinese invention patent CN105290418B discloses a plating method for plating a thick tin layer with a solderable thickness on the surface of a micro-nano copper ball, and obtains a Cu / Ag / Ni@Sn core-shell structure bimetallic powder with a thick tin layer on the surface. The composite preformed solder sheet can achieve low-temperature welding, and the obtained solder joint can withstand high melting point service. However, since the solder sheet is made by chemical plating, the plating solution has insufficient reduction ability or poor stability, the solution composition is complex, the process is complicated, the time required is long, and the maintenance of the solution is relatively troublesome.
[0007] Therefore, existing welding materials cannot meet the requirements of simple composition and process, strong reliability (welding stability), large-scale production, low-temperature interconnection in a short time, and high melting point service. Summary of the invention
[0008] In order to overcome the technical problems that the existing welding materials in the prior art cannot meet the requirements of simple composition and process, strong reliability, large-scale production, low-temperature interconnection and high melting point service in a short time.
[0009] The present invention proposes a packaging welding sheet, which not only has the characteristics of "low temperature welding and high temperature service", but also does not require the addition of additives or adhesives. Through the molding pressure of direct molding, micron-sized metal particles are evenly embedded in the rolled sheet formed by alloy solder powder, and are quickly formed into a packaging welding sheet with metal particles. The components and processes used are simple, the reliability is strong, and large-scale production is possible.
[0010] Specifically, the present invention discloses a packaging welding sheet, comprising alloy solder powder and micron-sized metal particles; the weight ratio of the alloy solder powder to the micron-sized metal particles is 8:1-1:1; the second melting point of the micron-sized metal particles is 3-8 times the first melting point of the alloy solder powder; the ratio of the average particle size of the alloy solder powder to the average particle size of the micron-sized metal particles is 0.5-1.5; the alloy solder powder and the micron-sized metal particles are mixed and molded once to obtain a packaging welding sheet; wherein, after the alloy solder powder is compacted, it is connected as a whole due to intermolecular forces to form a rolled sheet, so that the micron-sized metal particles are evenly embedded in the rolled sheet.
[0011] In the package welding sheet of the present invention, the addition of micron-sized metal particles can greatly increase the melting point of the package welding sheet. In the welding process, the package welding sheet first melts the alloy solder powder, and then undergoes a liquid-solid interdiffusion reaction with the micron-sized metal particles to form high-temperature resistant intermetallic compounds (IMCs), thereby achieving the effect of "low-temperature welding and high-temperature service". There is no need to add additives or adhesives. The mold pressure of direct molding is used to make the micron-sized metal particles evenly embedded in the rolled sheet formed by the alloy solder powder, and the package welding sheet with metal particles is quickly formed. The operation is simple and the cost is low. In addition, since the micron-sized metal particles can be evenly embedded in the rolled sheet, the package welding sheet has strong structural stability and welding stability.
[0012] Preferably, the upper and lower surfaces of the packaging welding sheet are covered or plated with at least one solder layer, and the solder layer is used to cover the exposed portions of the micron-sized metal particles on the upper and lower surfaces of the packaging welding sheet.
[0013] Preferably, the method for attaching or plating the solder layer on the upper and lower surfaces of the packaging welding sheet is to attach a prefabricated solder sheet to the rolled sheet, and perform secondary molding on the rolled sheet with the solder sheet attached to form the solder layer.
[0014] Preferably, the solder layer is configured as an alloy solder powder layer or a tin solder layer.
[0015] Preferably, the micron-sized metal particles are configured as mixed metal particles; or the micron-sized metal particles are configured as alloy particles; or the micron-sized metal particles are configured as plated metal particles.
[0016] Preferably, at least one layer of flux is sprayed on the upper and lower surfaces of the packaging welding piece; or at least one layer of solder layer is pasted or plated on the upper and lower surfaces of the packaging welding piece, and at least one layer of flux is sprayed on the upper and lower surfaces of the solder layer.
[0017] The packaging welding piece is covered / plated with a solder layer on the surface to cover the micron-sized metal particles exposed on the surface. The provision of the solder layer is beneficial to improving the fit between the packaging welding piece and the material to be welded during welding, and avoids the problem of loose welding joints caused by voids between the welding piece and the substrate.
[0018] During the soldering reflow process, the solder layer at the soldering interface will melt first and react with the substrate, greatly improving the wettability of the solder piece to the substrate. At the same time, the melted solder layer will also react with the alloy solder powder in the solder piece, so that the weld forms a multi-layer structure and is tightly connected.
[0019] Furthermore, the multiple pressure forming (compression molding) process of the packaging welding sheet of the present invention ensures its dense structure and product qualification rate, so that the weld is tight and the interface connection is dense in the subsequent welding, and the strength and toughness of the composite intermetallic compound formed by the welding joint are unified, and it has excellent comprehensive mechanical properties.
[0020] Preferably, the alloy solder powder is a mixture of one or more of tin-based alloy powder, indium-based alloy powder or bismuth-based alloy powder.
[0021] Preferably, the tin-based alloy powder is a mixture of one or more of Sn96.5Ag3.5, Sn99.3Cu0.7, Sn77.2In20Ag2.8; the indium-based alloy powder is a mixture of one or more of In97Ag3 or In52Sn48; the bismuth-based alloy powder is a mixture of one or more of Bi58Sn42 or Bi57Sn42Ag1.
[0022] Preferably, the alloy solder powder can be prepared into nano alloy solder powder by liquid phase chemical reduction method or consumable electrode DC arc method; or the micron-sized metal particles can be prepared into nano metal particles by high energy ball milling method. The package solder sheet made of nano alloy solder powder and nano metal particles has a more compact structure, and its strength and toughness can be enhanced.
[0023] The present invention also discloses a method for preparing the above-mentioned packaging solder sheet, comprising the following steps:
[0024] S1: screening the alloy solder powder and micron-sized metal particles respectively;
[0025] S2: fully mixing the screened alloy solder powder and the micron-sized metal particles and then ball milling them to form a mixed powder;
[0026] S3: Molding the mixed powder to form a packaging solder sheet. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying any creative work.
[0028] Figure 1 1 is a side view of the package solder sheet (including the solder layer and the flux layer) of Example 1.
[0029] In the figure: 1- micron-sized metal particles; 2- alloy solder powder; 3- solder layer; 4- flux layer. DETAILED DESCRIPTION
[0030] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.
[0032] It should also be understood that the terms used in this specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the specification of the present invention and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.
[0033] It should be further understood that the term "and / or" used in the present description and the appended claims refers to any and all possible combinations of one or more of the associated listed items, and includes these combinations.
[0034] In addition, the terms "roughly" and "basically" are intended to explain that the relevant content does not require absolute precision, but can have certain deviations. For example, "roughly equal" does not only mean absolute equality. Since it is difficult to achieve absolute "equality" in actual production and operation, there are generally certain deviations. Therefore, in addition to absolute equality, "roughly equal" also includes the above-mentioned situation with certain deviations. Taking this as an example, in other cases, unless otherwise specified, the terms "roughly" and "basically" have similar meanings to the above.
[0035] A packaging welding sheet comprises alloy solder powder and micron-sized metal particles, wherein the weight ratio of the alloy solder powder to the micron-sized metal particles is 8:1-1:1.
[0036] The alloy solder powder and a plurality of micron-sized metal particles are mixed and molded once to obtain a packaging solder sheet; wherein, after the alloy solder powder is compacted, it is connected as a whole due to the intermolecular force to form a rolled sheet, so that the plurality of micron-sized metal particles are evenly embedded in the rolled sheet, that is, the alloy solder powder is connected as a whole under the action of the molding pressure, and the micron-sized metal particles will not deform at this time, so they are squeezed into various gaps in the rolled sheet, so that the plurality of micron-sized metal particles are evenly integrated into the alloy solder powder to form a rolled sheet.
[0037] A solder sheet with controllable solder joint thickness according to an embodiment of the present invention (comprising a solder layer and a flux layer) is as follows: Figure 1 As shown, under the effect of the mold pressure, the alloy solder powder 2 is rolled into one body to form a rolled sheet, and the micron-sized metal particles 1 are evenly distributed in the gaps in the rolled sheet to form a rolled sheet.
[0038] Post-processing can also be performed on the rolled sheet to add a solder layer 3 and / or a flux layer 4, specifically, Figure 1 The rolled sheet also includes a solder layer 3 and a flux layer 4.
[0039] The micron-sized metal particles are selected from at least one of Ag, Cu and Ni, and the alloy solder powder is a mixture of one or more of tin-based solder, indium-based solder and bismuth-based solder.
[0040] According to the molecular weight of most tin-based solders, indium-based solders, bismuth-based solders, as well as Ag, Cu, and Ni, when the weight of the alloy solder powder is relatively large, the content of micron-sized metal particles will be relatively small, which will affect the generation of intermetallic compounds (IMCs). When the weight of the alloy solder powder is relatively small, the micron-sized metal particles have relatively poor ductility, high hardness and brittleness, which will make it difficult to form the package solder sheet or prone to cracks. Therefore, the weight of the micron-sized metal particles usually does not exceed the weight of the alloy solder powder.
[0041] The second melting point of the micron-sized metal particles is 3-8 times the first melting point of the alloy solder powder. Since metal particles such as Ag, Cu, and Ni have relatively high melting points, for example, the melting point of Ag is about 961.93°C, the melting point of Cu is about 1083.4°C, and the melting point of Ni is about 1453°C, the melting point of pure tin is 231.9°C, the melting point of pure indium is 156.51°C, and the melting point of pure bismuth is 271.5°C. The melting point of tin-based solder varies depending on the combination of tin with different alloys, and the preferred range is usually about 200-350°C. The melting point of indium-based solder varies depending on the combination of indium with different alloys, and the preferred range is usually about 150-250°C. The melting point of bismuth-based solder varies depending on the combination of bismuth with different alloys, and the preferred range is usually about 250-400°C.
[0042] It can be seen that the melting point range of micron-sized metal particles is about 900-1500°C, and the melting point range of alloy solder powder is about 150-400°C, that is, the first melting point of micron-sized metal particles is 3-10 times the second melting point of alloy solder powder.
[0043] The ratio of the average particle size of the alloy solder powder to the average particle size of the micron-sized metal particles is 0.5-1.5, which can effectively ensure that the alloy solder powder and the micron-sized metal particles can be fully mixed. The purpose of setting this particle size ratio is to allow the alloy solder powder and the micron-sized metal particles to be fully mixed. Because if the average particle size of the alloy solder powder is too different from the average particle size of the micron-sized metal particles, the small particles will sink to the bottom of the large particles under the action of gravity. After rolling, it is easy to cause stratification of the alloy solder powder and the micron-sized metal particles. Usually, the small-diameter particles will fall to the bottom and cannot be fully mixed.
[0044] Therefore, in actual selection, it is usually selected that the average particle size of the alloy solder powder is consistent with that of the micron-sized metal particles or the average particle size of the alloy solder powder is slightly larger than that of the micron-sized metal particles. Preferably, the average particle size of the micron-sized metal particles is preferably 5-25 μm, and the average particle size of the alloy solder powder is preferably 10-40 μm. Too small alloy solder powder and micron-sized metal particles will make the particle specific surface area too large, and the surface is easily oxidized, resulting in subsequent poor welding. Too large alloy solder powder and micron-sized metal particles are likely to cause insufficient metallurgical bonding, and are likely to cause local enrichment of alloy solder powder and micron-sized metal particles.
[0045] The alloy solder powder and a plurality of micron-sized metal particles are mixed and molded once to obtain a packaging solder sheet; wherein, after the alloy solder powder is compacted, it is connected as a whole due to the intermolecular force to form a rolled sheet, so that the plurality of micron-sized metal particles are evenly embedded in the rolled sheet, that is, the alloy solder powder is connected as a whole under the action of the molding pressure, and the micron-sized metal particles do not deform at this time, so they are squeezed into the gaps of the rolled sheet, so that the plurality of micron-sized metal particles are evenly integrated into the alloy solder powder to form a rolled sheet.
[0046] Since the micron-sized metal particles are selected from Ag, Cu, and Ni, they are relatively hard and difficult to deform, while the alloy solder powder is selected from one or more of tin-based solder, indium-based solder, or bismuth-based solder, which is relatively soft and easy to deform. Preferably, the hardness of the alloy solder powder is less than the hardness of the micron-sized metal particles. Therefore, it is only necessary to control the molding pressure of the hydraulic molding machine to a pressure corresponding to the intermolecular force generated by the alloy solder powder to deform and form a rolled sheet. At this time, the micron-sized metal particles can withstand this molding pressure without deformation or with very little deformation, that is, the pressure corresponding to the deformation of the alloy solder powder is less than the working pressure of the molding machine, which is less than the pressure corresponding to the deformation of the micron-sized metal particles.
[0047] In actual production, the molding pressure can be reasonably selected according to the deformation characteristics of different solders such as tin-based solder, indium-based solder or bismuth-based solder. For example, the molding pressure of bismuth-based solder is preferably controlled at 30-65Mpa. The addition of micron-sized metal particles can greatly increase the melting point of the package solder piece. During the welding process, the package solder piece will first melt the alloy solder powder, and then undergo liquid-solid interdiffusion reaction with the micron-sized metal particles to form high-temperature resistant intermetallic compounds (IMCs), thereby achieving the effect of "low-temperature welding and high-temperature service".
[0048] The packaging solder sheet does not require the addition of additives or adhesives. Through direct molding pressure, the micron-sized metal particles are evenly embedded in the rolled sheet formed by the alloy solder powder, and are quickly formed into a packaging solder sheet with metal particles. The operation is simple and the cost is low. Moreover, since the micron-sized metal particles can be evenly embedded in the rolled sheet and are difficult to fall off from the alloy solder powder, the packaging solder sheet has strong structural stability and welding stability.
[0049] The upper and lower surfaces of the package welding piece are covered / plated with at least one layer of solder layer. Preferably, a layer of solder layer is usually provided, and the solder layer is used to cover the exposed micron-sized metal particles on the upper and lower surfaces of the package welding piece. The solder layer covers the exposed micron-sized metal particles on the surface to prevent the micron-sized metal particles from adversely affecting the flow of the solder liquid. The solder layer is conducive to improving the fit between the package welding piece and the material to be welded during welding, and avoids the problem of weak welding joints caused by voids between the welding piece and the substrate.
[0050] During the soldering reflow process, the solder layer at the soldering interface will first melt and react with the substrate, greatly improving the wettability of the solder sheet to the substrate. At the same time, the melted solder layer will also react with the alloy solder powder in the solder sheet, so that the weld forms a multi-layer structure and is tightly connected. Further preferably, in actual production, the solder sheet can be prefabricated first, the prefabricated solder sheet is attached to the rolled sheet, and the rolled sheet with the solder sheet attached is subjected to secondary molding to form a solder layer. This packaged solder sheet undergoes multiple pressure molding processes to ensure its dense structure and product qualification rate, so that the weld is tight and the interface connection is dense in subsequent welding, and the strength and toughness of the composite intermetallic compound formed by the weld joint are unified, and it has excellent comprehensive mechanical properties.
[0051] Further preferably, the solder layer is configured as an alloy solder powder layer or a tin solder layer. Of course, an indium solder layer or a bismuth solder layer can also be selected. Bismuth solder layers are relatively rare, but this application does not limit this. Just select a solder with good wettability. In actual production, in order to solve cost problems and maintain product consistency, it is preferred to configure the solder layer as an alloy solder powder layer or a tin solder layer, so as to ensure that the prepared package solder sheet has good wettability and is also conducive to reducing the production cost of the package solder.
[0052] The micron-sized metal particles are configured as mixed metal particles or the micron-sized metal particles are configured as alloy particles or the micron-sized metal particles are configured as plated metal particles. The micron-sized metal particles are selected from at least one of Ag, Cu, and Ni; when two or more micron-sized metal particles are selected, mixed metal particles are formed; when alloy balls composed of two elements of Ag, Cu, and Ni are selected, alloy particles are formed; when another element is plated on the outer surface of an element, for example: Ag is plated on the outer surface of a Cu ball, plated metal particles are formed. Regardless of which of the above particles the micron-sized metal particles are configured as, it is applicable to this embodiment. The micron-sized metal particles screened in this embodiment need to meet the technical feature of "the pressure corresponding to the deformation of the alloy solder powder < the working pressure of the molding machine < the pressure corresponding to the deformation of the micron-sized metal particles" and the metal particles are micron-sized to ensure that they are evenly distributed in the alloy solder powder.
[0053] The alloy solder powder is preferably a mixture of one or more of tin-based alloy powder, indium-based alloy powder or bismuth-based alloy powder. The tin-based alloy powder is preferably a mixture of one or more of Sn96.5Ag3.5, Sn99.3Cu0.7, Sn77.2In20Ag2.8 (specifically, in Sn96.5Ag3.5, the mass content of Sn is 96.5%, the mass content of Ag is 3.5%, and other similar alloy expressions are the same); the indium-based alloy powder is preferably a mixture of one or more of In97Ag3 or In52Sn48; the bismuth-based alloy powder is selected as a mixture of one or more of Bi58Sn42 or Bi57Sn42Ag1. However, no matter what kind of alloy solder the alloy solder powder is, the melting point range of the alloy solder powder is about 150-400°C, and it also needs to meet the technical feature of "the pressure corresponding to the deformation of the alloy solder powder < the working pressure of the molding machine < the pressure corresponding to the deformation of the micron-sized metal particles".
[0054] In order to prevent oxidation of the rolled sheet and improve the welding effect, at least one layer of flux is sprayed on the upper and lower surfaces of the package welding sheet, or at least one layer of solder layer is attached / plated on the upper and lower surfaces of the package welding sheet, and at least one layer of flux is sprayed on the upper and lower surfaces of the solder layer. The sprayed flux forms a flux layer on the outer surface of the rolled sheet to improve the welding effect. The flux is configured as a mixture of one or more of inorganic flux, organic flux and rosin-type flux. In actual production, 0.5-1.5% flux is usually sprayed on the outer surface of the rolled sheet, and the preferred ratio is 1%, so as to further improve the welding performance of the welding sheet.
[0055] A method for preparing the above-mentioned packaging solder sheet comprises the following steps:
[0056] S1: The alloy solder powder and micron-sized metal particles are screened respectively. The purpose of the screening is to screen the alloy solder powder and micron-sized metal particles with suitable particle sizes. Preferably, the average particle size of the micron-sized metal particles is preferably 5-25 μm, and the average particle size of the alloy solder powder is preferably 10-40 μm.
[0057] Specifically, the melting point, average particle size and hardness of the alloy solder powder and micron-sized metal particles need to be selected according to customer needs, so that the micron-sized metal particles are evenly distributed in the rolled sheet of the alloy solder powder. The average particle size of the alloy solder powder and micron-sized metal particles is controlled within a reasonable range by setting the pore size of the screening machine. Of course, it is difficult to determine the specific size of each alloy solder powder and micron-sized metal particle in actual production, but the screening machine can be used to ensure that the average particle size of the particles is consistent or nearly consistent.
[0058] S2: The screened alloy solder powder and the micron-sized metal particles are fully mixed and ball-milled to form a mixed powder. In step S2, the purpose of ball milling is to fully mix the alloy solder powder and the metal particles so that the micron-sized metal particles are distributed throughout the alloy solder powder, which is conducive to the formation of intermetallic compounds (IMCs), especially full IMCs, in the subsequent use of the package solder sheet.
[0059] During the mixing process, the weight ratio of the alloy solder powder and the micron-sized metal particles is preferably 8-1:1, and more preferably, the weight ratio is 3.5:1-2; this is conducive to the rapid formation of the IMC structure during welding, which not only enhances the solder strength, but also greatly improves the electrical and thermal conductivity of the package solder piece. Taking tin-based alloy powder and copper-containing micron-sized metal particles as an example, a large proportion of Cu particles will generate the metal compound Cu3Sn, affecting the weldability, and a small proportion of Cu particles cannot form IMC, and the reaction time is slow. Therefore, it is necessary to reasonably control the weight ratio of the alloy solder powder and the micron-sized metal particles.
[0060] Preferably, the ball milling parameters are: the rotation speed is 150-350RPM, the ball milling time is 3-8min; the ball milling tank and ball milling beads used are made of zirconia material that is not easy to wear. If the speed of the ball mill is too high or the ball milling time is too long, the alloy solder powder and the micron-sized metal particles are easily cold welded and agglomerated. If the speed of the ball mill is too low or the ball milling time is too short, it is easy to cause uneven mixing of the powder.
[0061] S3: Molding the mixed powder. In step S3, a package solder sheet is obtained after molding, wherein the alloy solder powder is compacted and connected as a whole to form a rolled sheet, and micron-sized metal particles are evenly filled in the rolled sheet to form a package solder sheet.
[0062] Specifically, the pressing pressure is controlled at 30-65Mpa during the molding process, and the pressure is maintained for 3-5 minutes, and the pressure strength and time are accurately controlled; preferably, the pressing pressure is controlled at 60Mpa during the molding process to make it more densely bonded and have high bonding strength. After the film is pressed, a 0.7-1mm package solder sheet is obtained.
[0063] After molding, the shape and thickness of the package welding sheet can be processed by rolling to obtain a package welding sheet with a thickness of 0.1-0.2mm. The deformation amount of each rolling is controlled within 10% to gradually roll the package welding sheet into a thinner strip material, and the final thickness is between 0.1-0.2mm.
[0064] The package solder sheet can also be sprayed with 0.5-1.5% halogen-free rosin soldering flux by weight on the upper and lower surfaces; the preferred ratio is 1wt%, which can be commercially available RL-420. Then, it is placed in a 60°C oven and baked for 20 minutes until the solvent in the soldering flux evaporates.
[0065] Repeat the coating process several times, and control the proportion of flux between 0.5-1.5% by weighing the weight before and after the flux. This step helps to remove the oxides generated on the surface of the package solder during the production process during the soldering process, and activates the solder surface so that it can quickly wet the substrate layer. At the same time, the dried flux does not contain solvents, which prevents the solvent from evaporating during the soldering process and forming gaps in the solder joints.
[0066] The packaging welding sheet can also be coated with a solder layer on the upper and lower surfaces. Specifically, a prefabricated solder sheet is attached to a rolled sheet, and the rolled sheet with the solder sheet attached is subjected to secondary molding to form a solder layer. The multiple pressure molding process of the packaging welding sheet ensures its dense structure and product qualification rate, so that the weld is tight and the interface connection is dense in subsequent welding. The composite intermetallic compound formed by the welding joint has the unity of strength and toughness, and has excellent comprehensive mechanical properties.
[0067] Finally, the preliminarily formed packaging solder piece can also be stamped to preset and adjust the shape of the packaging solder piece; preferably, a punch press is used for stamping to form a preformed packaging solder piece.
[0068] Example 1
[0069] A method for preparing a package solder sheet provided in this embodiment includes the following steps:
[0070] S1. Prepare raw materials: Divide Bi58Sn42 with average particle sizes of 5μm, 10μm, 20μm, 30μm, and 35μm into five groups: Group A, Group B, Group C, Group D, and Group E. Mix the five groups of Group A, Group B, Group C, Group D, and Group E with copper powder Cu with an average particle size of 20μm. Specifically, weigh the five groups of Bi58Sn42 powder and Cu powder at a weight ratio of 3.5:1, weigh 40g of Bi58Sn42 powder and 11.4g of Cu powder and mix them together. Among them, the first melting point of Bi58Sn42 powder is 255℃, the second melting point of Cu powder is 1084.6℃, and the melting point ratio of the first melting point to the second melting point is 4.3:1.
[0071] S2, ball milling and mixing: the raw materials mixed in step S1 are placed together with stainless steel balls in a stainless steel ball milling jar and then placed in a planetary ball mill for mixing. The ball milling speed is 200 RPM and the ball milling time is 5 min.
[0072] S3. Molding: Take out the mixed powders of group A, group B, group C, group D and group E respectively, and then put them into the mold respectively. The pressure is set to 40Mpa, and the pressure is maintained for 4 minutes to press them into five groups of rolled sheets (package welding sheets) with a thickness of 0.8mm, namely group A, group B, group C, group D and group E.
[0073] S4, rolling: the two-roll mill is heated to 110°C, the roll speed is set at 2m / min, and the rolled sheet is gradually rolled into five groups of thinner strips, namely, group A, group B, group C, group D, and group E, with a final thickness of 0.17mm.
[0074] S5, spraying flux: spray 0.8wt% flux (halogen-free rosin flux - commercially available RL-420) on both sides of the five groups of strips of material, group A, group B, group C, group D, and group E, and bake them in a 60°C oven for 20 minutes until the solvent in the flux evaporates. Repeat the coating process several times.
[0075] S6 punching and molding: The composite solder strip with surface coating / plating with flux is punched and molded by a punch press to obtain the final A group, B group, C group, D group, and E group packaging solder pieces.
[0076] Table 1 Stratification of Bi58Sn42 with different particle sizes mixed with copper powder
[0077] Group Whether to layer Group A Severe stratification, Bi58Sn42 powder is enriched at the bottom Group B A small amount of delamination, Bi58Sn42 powder is on the bottom Group C No obvious stratification Group D A small amount of stratification, Cu powder is on the bottom Group E Severe stratification, Cu powder is concentrated at the bottom
[0078] From the above experiments, it can be known that the greater the difference in the average particle size between Bi58Sn42 powder and Cu powder, the easier it is to cause uneven mixing of Bi58Sn42 powder and Cu powder. When the average particle size ratio of Bi58Sn42 powder to Cu powder is <0.5 or >1.5, there is an obvious stratification phenomenon, either the Bi58Sn42 powder sinks to the bottom or the Cu powder sinks to the bottom; when the average particle size ratio of Bi58Sn42 powder to Cu powder is 0.5≥ and ≤1.5, there is an acceptable small amount of stratification phenomenon. When the average particle size ratio of Bi58Sn42 powder to Cu powder is 1, there is no obvious stratification phenomenon. Therefore, preferably, if only the factor of mixing uniformity is considered, the average particle sizes of Bi58Sn42 powder and Cu powder are consistent or nearly consistent, so that the average particle sizes of Bi58Sn42 powder and Cu powder are fully mixed.
[0079] In addition to ensuring sufficient mixing, preferably, the average particle size of Cu powder is preferably 5-25μm, and the average particle size of Bi58Sn42 powder is preferably 10-40μm. Too small Bi58Sn42 powder and Cu powder will make the particle specific surface area too large, and the surface is easily oxidized, resulting in subsequent poor welding. Too large Bi58Sn42 powder and Cu powder are prone to insufficient metallurgical bonding and local enrichment of Bi58Sn42 powder and Cu powder.
[0080] In summary, Bi58Sn42 powder and Cu powder of appropriate sizes are usually selected, and the average particle size of Bi58Sn42 powder is preferably slightly larger than that of Cu powder to ensure that the Cu powder is evenly distributed in the rolled sheet of Bi58Sn42 powder.
[0081] Example 2
[0082] A method for preparing a package solder sheet provided in this embodiment includes the following steps:
[0083] S1. Prepare raw materials: Use bismuth-based alloy powder with an average particle size of 25μm and copper powder with an average particle size of 20μm to weigh Bi58Sn42 powder and Cu powder in a weight ratio of 3.5:1.5, and mix 35g of Bi58Sn42 powder and 10.5g of Cu powder together. Among them, the first melting point of Bi58Sn42 powder is 255℃, the second melting point of Cu powder is 1084.6℃, and the melting point ratio of the first melting point to the second melting point is 4.3:1.
[0084] S2, ball milling and mixing: the raw materials mixed in step S1 are placed together with stainless steel balls in a stainless steel ball milling jar and then placed in a planetary ball mill for mixing. The ball milling speed is 250 RPM and the ball milling time is 5 min.
[0085] S3. Molding: Take out the mixed powder, put it into the die, set the pressure to 40Mpa, keep the pressure for 4 minutes, and then press it into a calendered sheet with a thickness of 0.8mm.
[0086] S4, rolling: the two-roll mill is heated to 120℃, the roll speed is set at 2m / min, and the calendered sheet is gradually rolled into a thinner strip, with a final thickness of 0.17mm
[0087] S5. Spraying flux: Spray 1.5 wt% flux (halogen-free rosin flux - commercially available RL-420) evenly on both sides of the composite solder strip, and bake it in a 60° C. oven for 20 minutes until the solvent in the flux evaporates. Repeat the coating process several times.
[0088] S6 punching and molding: The composite solder strip with the surface coated / plated with flux is punched and molded by a punching machine to obtain the final package solder piece.
[0089] Example 3
[0090] A method for preparing a package solder sheet provided in this embodiment includes the following steps:
[0091] S1. Prepare raw materials: Use bismuth-based alloy powder with an average particle size of 25μm and copper powder with an average particle size of 20μm to weigh Bi58Sn42 powder and Ni powder in a weight ratio of 3.5:1.5, and mix 35g of Bi58Sn42 powder and 10.5g of Cu powder together. Among them, the first melting point of Bi58Sn42 powder is 255℃, the second melting point of Ni powder is 1453℃, and the melting point ratio of the first melting point to the second melting point is 5.7:1.
[0092] S2, ball milling and mixing: the raw materials mixed in step S1 are placed together with stainless steel balls in a stainless steel ball milling jar and then placed in a planetary ball mill for mixing. The ball milling speed is 250 RPM and the ball milling time is 5 min.
[0093] S3. Molding: Take out the mixed powder, put it into the die, set the pressure to 45Mpa, keep the pressure for 4 minutes, and then press it into a calendered sheet with a thickness of 0.8mm.
[0094] S4, rolling: the two-roll mill is heated to 120℃, the roll speed is set at 2m / min, and the calendered sheet is gradually rolled into a thinner strip, with a final thickness of 0.17mm
[0095] S5. Spraying flux: Spray 1.5 wt% flux (halogen-free rosin flux - commercially available RL-420) evenly on both sides of the composite solder strip, and bake it in a 60° C. oven for 20 minutes until the solvent in the flux evaporates. Repeat the coating process several times.
[0096] S6 punching and molding: The composite solder strip with the surface coated / plated with flux is punched and molded by a punching machine to obtain the final package solder piece.
[0097] Embodiment 4 to Embodiment 9
[0098] Example 4: Replace "Cu powder" in Example 2 with "Ag powder", and the rest of the steps are the same. The first melting point of Bi58Sn42 powder is 255°C, the second melting point of Ag powder is 961°C, and the melting point ratio of the first melting point to the second melting point is 3.8:1.
[0099] Example 5: Replace "Bi58Sn42 powder" in Example 2 with "Bi57Sn42Ag1 powder", and the remaining steps are the same. The first melting point of Bi57Sn42Ag1 powder is 262°C, the second melting point of Cu powder is 1084.6°C, and the melting point ratio of the first melting point to the second melting point is 4.1:1.
[0100] Example 6: Replace "Bi58Sn42 powder" in Example 2 with "In52Sn48 powder", and the remaining steps are the same. The first melting point of In52Sn48 powder is 179°C, the second melting point of Cu powder is 1084.6°C, and the melting point ratio of the first melting point to the second melting point is 6.1:1.
[0101] Example 7: Replace "Bi58Sn42 powder" in Example 2 with "In97Ag3 powder", and the remaining steps are the same. The first melting point of In97Ag3 powder is 181°C, the second melting point of Cu powder is 1084.6°C, and the melting point ratio of the first melting point to the second melting point is 6:1.
[0102] Example 8: Replace "Bi58Sn42 powder" in Example 2 with "Sn77.2In20Ag2.8", and the remaining steps are the same. The first melting point of Sn77.2In20Ag2.8 powder is 237°C, the second melting point of Cu powder is 1084.6°C, and the melting point ratio of the first melting point to the second melting point is 4.6:1.
[0103] Example 9: Replace "Bi58Sn42 powder" in Example 2 with "Sn96.5Ag3.5", and the rest of the steps are the same. The first melting point of Sn96.5Ag3.5 powder is 258°C, the second melting point of Cu powder is 1084.6°C, and the melting point ratio of the first melting point to the second melting point is 4.2:1.
[0104] Table 2 Performance test results of Examples 2 to 9
[0105]
[0106]
[0107] It can be seen from the above table that the melting point, electrical conductivity and thermal conductivity of the packaging welding piece provided in this embodiment are improved. Compared with pure Bi58Sn42, the packaging welding piece provided in Examples 2-9 has a higher proportion of IMCs during welding. During the welding process, this packaging welding piece first melts the alloy solder powder, and then undergoes liquid-solid interdiffusion reaction with the micron-sized metal particles to form high-temperature resistant intermetallic compounds (IMCs), thereby achieving the effect of "low-temperature welding, high-temperature service".
[0108] The main processing method of the packaging welding sheet provided in Example 2-9 is molding, and the subsequent rolling and stamping are only for further generating a "prefabricated welding sheet". During the processing, no additives or adhesives are required in the production of the "prefabricated welding sheet". The molding pressure of direct molding is used to make the micron-sized metal particles evenly embedded in the rolled sheet formed by the alloy solder powder, and quickly formed into a packaging welding sheet with metal particles.
[0109] Example 10
[0110] A method for preparing a package solder sheet provided in this embodiment includes the following steps:
[0111] S1. Prepare raw materials: Use bismuth-based alloy powder with an average particle size of 25μm and copper powder with an average particle size of 20μm to weigh Bi58Sn42 powder and Cu powder in a weight ratio of 3.5:1.5, and mix 35g of Bi58Sn42 powder and 10.5g of Cu powder together. Among them, the first melting point of Bi58Sn42 powder is 255℃, the second melting point of Cu powder is 1084.6℃, and the melting point ratio of the first melting point to the second melting point is 4.3:1.
[0112] S2, ball milling and mixing: the raw materials mixed in step S1 are placed together with stainless steel balls in a stainless steel ball milling jar and then placed in a planetary ball mill for mixing. The ball milling speed is 250 RPM and the ball milling time is 5 min.
[0113] S3, one-time molding: take out the mixed powder, put it into the molding, set the pressure to 40Mpa, keep the pressure for 4 minutes, and then press it into a calendered sheet with a thickness of 0.8mm.
[0114] S4. Secondary molding: prefabricate Bi58Sn42 powder sheets, that is, prefabricate solder sheets, attach the prefabricated Bi58Sn42 powder sheets to the rolled sheets, perform secondary molding on the rolled sheets with Bi58Sn42 powder sheets attached, form solder layers attached to the upper and lower surfaces of the rolled sheets, and form a composite rolled sheet.
[0115] S5, rolling: the two-roll mill is heated to 120°C, the roll speed is set at 2m / min, and the composite rolled sheet is gradually rolled into a thinner strip, with a final thickness of 0.17mm.
[0116] S6, spraying flux: spray 1.5wt% flux (halogen-free rosin flux - commercially available RL-420) evenly on both sides of the strip, place in a 60°C oven and bake for 20 minutes until the solvent in the flux evaporates. Repeat the coating process several times.
[0117] S7 punching and molding: The composite solder strip with the surface coated / plated with flux is punched and molded by a punching machine to obtain the final package solder piece.
[0118] Table 3 Performance test results of Example 2 and Example 10
[0119]
[0120]
[0121] It can be seen from the above table that after the packaging welding piece provided by the present invention is coated / plated with a solder layer on the surface, the melting point, electrical conductivity and thermal conductivity of the packaging welding piece will be slightly reduced, but its wettability will be greatly improved. The provision of a solder layer is beneficial to improving the fit between the packaging welding piece and the material to be welded during welding, avoiding the problem of loose welding joints caused by voids between the welding piece and the substrate. During the welding reflow process, the solder layer at the welding interface will melt first and react with the substrate, greatly improving the wettability of the welding piece to the substrate.
[0122] In addition, Example 10 is formed by multi-layer molding or rolling, so that the solder layer also reacts with the alloy solder powder in the solder sheet during soldering, so that the weld forms a multi-layer structure and is tightly connected. Furthermore, the multiple pressure forming process of the package solder sheet provided by the present invention ensures its dense structure and product qualification rate, so that the weld is tight and the interface connection is dense in subsequent welding, and the strength and toughness of the composite intermetallic compound formed by the welding joint are unified, and it has excellent comprehensive mechanical properties.
[0123] The present invention is described by preferred embodiments, and those skilled in the art will appreciate that various changes or equivalent substitutions may be made to these features and embodiments without departing from the spirit and scope of the present invention. The present invention is not limited to the specific embodiments disclosed herein, and other embodiments falling within the claims of this application are within the scope of protection of the present invention.
Claims
1. A package solder sheet, Features: Including alloy solder powder, and micron-sized metal particles; The weight ratio of the alloy solder powder to the micron-sized metal particles is 8:1-1:1; The second melting point of the micron-sized metal particles is 3-8 times the first melting point of the alloy solder powder; The ratio of the average particle size of the alloy solder powder to the average particle size of the micron-sized metal particles is 0.5-1.5; The hardness of the alloy solder powder is less than the hardness of the micron-sized metal particles; The alloy solder powder and the micron-sized metal particles are mixed and molded once to obtain a packaging solder sheet; wherein, the pressure corresponding to the deformation of the alloy solder powder is less than the working pressure of the molding machine and less than the pressure corresponding to the deformation of the micron-sized metal particles. After the alloy solder powder is compacted, it is connected as a whole due to the intermolecular force to form a rolled sheet, so that the micron-sized metal particles are evenly embedded in the rolled sheet.
2. The packaging solder sheet according to claim 1, Features: The upper and lower surfaces of the packaging welding piece are covered or plated with at least one solder layer, and the solder layer is used to cover the exposed parts of the micron-sized metal particles on the upper and lower surfaces of the packaging welding piece.
3. The packaging solder sheet according to claim 2, Features: The method for attaching or plating the solder layer on the upper and lower surfaces of the packaging welding sheet is to attach a prefabricated solder sheet to the rolled sheet, and perform secondary molding on the rolled sheet with the solder sheet attached to form the solder layer.
4. The packaging solder sheet according to claim 2 or 3, Features: The solder layer is configured as an alloy solder powder layer or a tin solder layer.
5. The packaging solder sheet according to claim 1 or 2, Features: configuring the micron-sized metal particles as mixed metal particles; or configuring the micron-sized metal particles into alloy particles; or The micron-sized metal particles are configured as plated metal particles.
6. The packaging solder sheet according to claim 2, Features: At least one layer of soldering flux is sprayed on the upper and lower surfaces of the package solder sheet; or The upper and lower surfaces of the packaging welding sheet are covered or plated with at least one layer of solder layer, and the upper and lower surfaces of the solder layer are sprayed with at least one layer of flux.
7. The packaging solder sheet according to claim 1, Features: The alloy solder powder is a mixture of one or more of tin-based alloy powder, indium-based alloy powder or bismuth-based alloy powder.
8. The packaging solder sheet according to claim 7, Features: The tin-based alloy powder is a mixture of one or more of Sn96.5Ag3.5, Sn99.3Cu0.7, Sn77.2In20Ag2.8; The indium-based alloy powder is a mixture of one or more of In97Ag3 or In52Sn48; The bismuth-based alloy powder is one or a mixture of Bi58Sn42 or Bi57Sn42Ag1.
9. The packaging solder sheet according to claim 1, Features: The alloy solder powder is prepared into nano alloy solder powder by liquid phase chemical reduction method or consumable electrode DC arc method; or The micron-sized metal particles are prepared into nano-sized metal particles by high-energy ball milling.
10. A method for preparing the package solder sheet according to claim 1, It is characterized in that The following steps are involved: S1: screening the alloy solder powder and micron-sized metal particles respectively; S2: fully mixing the screened alloy solder powder and the micron-sized metal particles and then ball milling them to form a mixed powder; S3: Molding the mixed powder to form a packaging solder sheet.
Citation Information
Patent Citations
A tin-based solder / copper particle composite solder that can rapidly form high-temperature solder joints at low temperatures
CN104625466B
A plating method for plating a thick tin layer with a solderable thickness on the surface of micro-nano copper balls
CN105290418B
Low-temperature composite soldering paste and preparation method and using method thereof
CN103071943A
Nanoscale / micron size particle mixing type lead-free solder paste with size effect and manufacturing method thereof
CN103639614A
Soldering lug for soft soldering and power module assembly structure
CN103769764A