A kind of anti-fouling protective layer coating, anti-fouling INS membrane and preparation method
Through the stain-resistant protective layer coating combined with polycarbonate polyol resin and nano powder, the existing light-transmitting diaphragm has insufficient scratch resistance and solvent resistance, and has achieved stain resistance, scratch resistance and cosmetic resistance and improve sweat resistance and reduce production costs.
Patent Information
- Application Number
- CN202311292748.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-09-28
AI Technical Summary
The existing light-transmitting diaphragms are affected by the scratch resistance and solvent resistance of the transparent layer of PMMA or PC, and the cost is high, and the organic fluorine or silicone modified resin is optimized in cost and the adhesion matching of the adhesive force of the adhesive. There are challenges in the aspects.
The stain-resistant protective layer coating is used to combine polycarbonate polyol resin with nano powders to improve the dispersion of nano powders through surfactants, form a micro-nano structure to improve stain-resistant performance, and use chain extenders, curing agents and catalysts. Adjust the softness and hardness of the protective layer, and combine hydroxyacrylic resin to improve the adhesive performance of the ink layer.
It has achieved improvements in stain resistance, scratch resistance, cosmetics resistance and sweat resistance, reducing production costs, and improving the user experience and economic value of the diaphragm.
Smart Images

Figure CN117327438B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of INS decorative films, and in particular relates to a stain-resistant protective layer coating, a stain-resistant INS film and a preparation method thereof. Background Art
[0002] INS technology is the abbreviation of Film Insert Molding, also known as the film insert molding process. It prefabricates a patterned film and covers the surface of the part during the injection molding process, so that the surface of the part presents different colors and textures, and the appearance of the part can be quickly adjusted as needed. The film prepared by INS technology has the advantages of high clarity, diverse patterns, and beautiful product appearance. It is currently widely used in the fields of automotive decorative film, home appliance decorative film, toy decorative film, etc., especially in automotive interior film, which can effectively improve the refinement and added value of the product.
[0003] In the prior art, patent CN109016712A discloses a light-transmitting film, which includes a transparent film layer, a decorative layer, an adhesive layer and a plastic sheet layer, wherein the transparent film layer is a PMMA or PC layer, and the transparent film layer plays a protective role, protecting the decorative layer from being damaged. However, the light-transmitting film disclosed in the patent has no scratch resistance and solvent resistance because the transparent layer PMMA or PC layer has no water contact angle of <90° and no stain resistance, which will seriously affect the service life of the film, and the price of PMMA or PC film is high, and the use of these two films will greatly increase the production cost of the product.
[0004] In order to increase its stain resistance, the prior art uses a combination of fluorinated acrylate and photocurable resin (CN110922887A), a combination of polyurethane acrylic resin and organic fluorine modified resin (CN115584199A), or a combination of polyurethane acrylic resin and organic silicon modified acrylic resin (CN113249026A), and prepares a protective layer by coating, drying and curing. However, the above patents all use organic fluorine modified or organic silicon modified resins to increase their stain resistance. In actual use, considering cost optimization and matching of subsequent application processes, organic fluorine or organic silicon modified resins are not preferred. At the same time, resin modification will also affect the adhesion between the protective layer and the ink layer. Summary of the invention
[0005] In view of one or more of the above defects or improvement needs of the prior art, the present invention provides a stain-resistant protective layer coating, a stain-resistant INS membrane and a preparation method. The stain-resistant INS membrane has good stain resistance, as well as good scratch resistance, cosmetics resistance, sweat resistance and solvent resistance.
[0006] According to one aspect of the present invention, there is provided a stain-resistant protective layer coating, comprising the following components in parts by weight:
[0007] 80-120 parts of polycarbonate polyol resin, 20-50 parts of hydroxy acrylic resin, 2-12 parts of chain extender, 1-20 parts of curing agent, 0.1-2 parts of catalyst, 0.2-5 parts of nano powder, 1-8 parts of surfactant and 80-150 parts of solvent.
[0008] Polycarbonate polyol is the raw material for synthesizing a new generation of polycarbonate polyurethane. Compared with polyurethane materials synthesized by traditional polyols (such as ordinary polyesters, polyethers, etc.), polycarbonate polyurethane has better mechanical properties, hydrolysis resistance, heat resistance, oxidation resistance, friction resistance and chemical resistance. The inventors have found through research that the polyurethane formed by combining polycarbonate polyol resin with nanopowder can improve solvent wiping resistance and stain resistance. Because the polymer chain in polycarbonate polyol is a saturated aliphatic carbonate chain, it has the characteristics of low surface energy; the surface of nanopowder interacts with carbonate functional groups, and the surface of the film after coating into a protective layer can form a micro-nano structure of roughness, further amplifying the low surface energy performance of the material, thereby achieving the purpose of improving its stain resistance.
[0009] However, the dispersion performance of nanopowders in coatings is not good, resulting in poor leveling during coating, uneven thickness of the protective layer, and limited improvement in stain resistance. Nanopowder particles have extremely high specific surface area. When mixed with resin materials, there is a large interface and interfacial energy between the surface of the powder particles and the dispersion medium. This highly dispersed multiphase system is a thermodynamically unstable system. The particles always tend to agglomerate with each other and reduce the surface free energy, which leads to the destruction of the suspension system and the deterioration of the dispersion and stability of the entire system.
[0010] Suitable surfactants can significantly reduce the surface tension of the particle surface and the dispersion medium, and enhance wettability, which will increase the strength and thickness of the solvation film on the surface of the powder particles, improve the repellency of the solvation film, and thus improve the dispersibility and stability of the nanopowder in the resin. The inventors further found that adding an organic modified siloxane auxiliary agent (surfactant) to the protective layer coating can well disperse the nanopowder in the coating; the prepared protective layer has improved resistance to reagent wiping and stain resistance, and the protective layer has a uniform appearance and feel.
[0011] In addition, hydroxy acrylic resin can improve the adhesion performance of coating and ink layers; chain extenders, curing agents, and catalysts can adjust the hardness of the protective layer, facilitating subsequent adjustment of the scope of application.
[0012] As a further improvement of the present invention, the polycarbonate polyol resin is a resin prepared from polycarbonate polyol. The polycarbonate polyol resin preferably includes one or more of aliphatic polycarbonate polyol, aromatic polycarbonate polyol or mixed polycarbonate polyol.
[0013] Exemplarily, the polycarbonate polyol includes but is not limited to polyhexylene carbonate diol, polyhexanediol carbonate-1,6-diol ester diol, polycaprolactone hexamethylene carbonate diol, polybutylene carbonate diol, polycyclohexanedimethanol carbonate-1,6-diol ester diol, polypentanediol carbonate-1,5-hexanediol carbonate-1,6-diol ester diol, polybutanediol carbonate-1,4-hexanediol carbonate-1,6-diol ester diol or polyoctanol carbonate-2-octanol ester diol.
[0014] As a further improvement of the present invention, the molecular weight Mn of the polycarbonate polyol is 500-5000, preferably 1000-3000, and more preferably 1500-2000; and / or the viscosity of the polycarbonate polyol resin at 25° C. is 1000-60000 cps.
[0015] As a further improvement of the present invention, the solid content of the hydroxy acrylic resin is 20-60%; and / or the viscosity of the hydroxy acrylic resin at 25° C. is 500-50000 cps.
[0016] As a further improvement of the present invention, the nanopowder includes but is not limited to one or more of fumed silica, nanoalumina, nanozirconium oxide, nanozinc oxide, nanoboron nitride, and titanium dioxide; and / or the particle size of the nanopowder is 2 to 200 nm, preferably 5 to 100 nm, and more preferably 10 to 50 nm.
[0017] As a further improvement of the present invention, the surfactant includes but is not limited to an organic modified siloxane auxiliary agent, specifically including one or more of Evonik 450, 410, 100 or BYK306, 307, 378;
[0018] As a further improvement of the present invention, the chain extender is selected from butanediol, ethylene glycol, diethylene glycol, hexanediol, glycerol, trimethylolpropane, pentaerythritol or one or more of polyether polyols; and / or,
[0019] The curing agent is an isocyanate containing a rigid structure, specifically an isocyanate containing an alicyclic or cycloaliphatic structure; and / or,
[0020] The catalyst includes but is not limited to one or more of tetramethylbutylene diamine, triethylene diamine, stannous octoate, dibutyltin dilaurate, lead octoate, cobalt octoate, iron octoate, zinc naphthenate, and tetraisobutyl titanate; and / or,
[0021] The solvent includes, but is not limited to, one or more of toluene, ethyl acetate, butanone, butyl ester and N,N-dimethylformamide.
[0022] According to a second aspect of the present invention, there is provided a stain-resistant INS membrane, the protective layer of which is prepared by using the stain-resistant protective layer coating.
[0023] As a further improvement of the present invention, the anti-fouling INS membrane comprises a protective layer, an ink layer, an adhesive layer and a substrate layer in sequence.
[0024] According to a third aspect of the present invention, there is provided a method for preparing the anti-fouling INS membrane, comprising the following steps:
[0025] Prepare a protective layer; place a polycarbonate polyol resin in a stirring device, add a solvent, a hydroxy acrylic resin, a curing agent, a chain extender, a catalyst, a nano powder and a surfactant in sequence, and stir evenly to form a protective layer coating; apply the protective layer coating on a PET carrier film by a micro-dimpled or slit extrusion coating method, and after drying and curing, form a protective layer;
[0026] The added amounts of the components in the protective layer coating are as follows: 80-120 parts of polycarbonate polyol resin, 20-50 parts of hydroxy acrylic resin, 2-12 parts of chain extender, 1-20 parts of curing agent, 0.1-2 parts of catalyst, 0.2-5 parts of nano powder, 1-8 parts of surfactant, and 80-150 parts of solvent, in parts by weight;
[0027] Printing an ink pattern on the protective layer to form an ink layer after curing;
[0028] Applying an adhesive on the ink layer to form an adhesive layer after curing; preferably, applying the adhesive using a micro-dimpled coating machine;
[0029] The protective layer, ink layer and adhesive layer form a thermal transfer film, and the thermal transfer film and the substrate layer are preferably thermally pressed and laminated using a thermal laminating machine, wherein the adhesive layer of the thermal transfer film is in contact with the substrate layer; the PET carrier film is peeled off, and the protective layer and the ink layer are bonded to the surface of the substrate layer under the action of the adhesive layer to form a stain-resistant INS film.
[0030] As a further improvement of the present invention, the polycarbonate polyol resin is a resin prepared from polycarbonate polyol; the polycarbonate polyol resin is a resin prepared from polycarbonate polyol. The polycarbonate polyol resin preferably includes one or more of aliphatic polycarbonate polyol, aromatic polycarbonate polyol or mixed polycarbonate polyol;
[0031] The nano powder includes one or more of fumed silicon dioxide, nano alumina, nano zirconium oxide and nano boron nitride;
[0032] The surfactant includes an organic modified silicone adjuvant.
[0033] In general, the above technical solution conceived by the present invention has the following beneficial effects compared with the prior art:
[0034] The anti-fouling INS membrane of the present invention has good anti-fouling effect under the synergistic effect of polyurethane formed by polycarbonate polyol, nanopowder and surfactant, and the membrane has good scratch resistance, cosmetics resistance, sweat resistance and solvent resistance, which can enhance the consumer's use experience.
[0035] The anti-fouling INS membrane of the present invention has a simple preparation method, low production cost and good economic value. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a schematic diagram of the anti-fouling INS membrane structure of an embodiment of the present invention;
[0037] In all the drawings, the same reference numerals represent the same technical features, specifically: 1 - protective layer, 2 - ink layer, 3 - adhesive layer, 4 - substrate layer. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0039] In order to better understand the anti-fouling INS membrane and preparation method of the present invention, the following specific examples are provided (unless otherwise specified, the raw materials involved in the embodiments of the present invention are all commercially available general materials):
[0040] Example 1
[0041] Place 80 parts of polycarbonate polyol resin in a stirring device, then add 100 parts of solvent, stir for 5 minutes, then add 40 parts of hydroxy acrylic resin, stir for 5 minutes, then add 3 parts of curing agent, stir for 5 minutes, then add 2 parts of chain extender, 0.2 parts of catalyst, 0.3 parts of nano alumina and 2 parts of surfactant in sequence, stir for 20 minutes, stir evenly to form a protective layer coating.
[0042] The preparation method of INS membrane includes the following steps:
[0043] A protective layer coating was applied on a 30 μm PET film using a micro-concave coating machine. The coating roller was a 45-line anilox roller. The oven temperature of the coating machine was 150°C and the coating speed was 10 m / min. The protective layer was formed after baking and curing.
[0044] According to market needs, different colors and texture patterns are designed, and the ink pattern is printed on the protective layer using a 10-color printing machine. The oven temperature is 100°C and the printing speed is 50m / min. After baking and curing, an ink layer is formed;
[0045] The adhesive is coated on the ink layer by using a micro-concave coating machine. The coating roller is a 90-line anilox roller. The oven temperature of the coating machine is 140°C and the coating speed is 20m / min. After baking and curing, an adhesive layer is formed. The film is a thermal transfer film.
[0046] The thermal transfer film and the substrate layer are hot-pressed and laminated by a thermal laminating machine, wherein the adhesive layer of the thermal transfer film is in contact with the substrate layer, the hot pressing temperature is 200°C, the hot pressing pressure is 5MPa, and the hot pressing laminating speed is 2m / min. The adhesive layer is activated under the action of temperature and pressure and is firmly bonded to the substrate layer. The PET film is peeled off, and the protective layer and the ink layer are bonded to the surface of the substrate layer under the action of the adhesive layer to form a stain-resistant INS film.
[0047] Example 2
[0048] 100 parts of polycarbonate polyol resin were placed in a stirring device, and then 130 parts of solvent were added, stirred for 5 minutes, 30 parts of hydroxy acrylic resin were added, stirred for 5 minutes, 7 parts of curing agent were added, stirred for 5 minutes, and then 6 parts of chain extender, 0.5 parts of catalyst, 0.6 parts of nano-alumina and 5 parts of surfactant were added in sequence, stirred for 20 minutes, and stirred evenly to form a protective layer coating. The preparation method of INS membrane is referred to Example 1.
[0049] Example 3
[0050] 120 parts of polycarbonate polyol resin are placed in a stirring device, and then 150 parts of solvent are added, stirred for 5 minutes, and then 50 parts of hydroxy acrylic resin are added, stirred for 5 minutes, and then 18 parts of curing agent are added, stirred for 5 minutes, and then 10 parts of chain extender, 1.2 parts of catalyst, 1.5 parts of nano-alumina and 8 parts of surfactant are added in sequence, stirred for 20 minutes, and stirred evenly to form a protective layer coating. The preparation method of INS membrane is referenced to Example 1.
[0051] Example 4
[0052] 90 parts of polycarbonate polyol resin are placed in a stirring device, and then 80 parts of solvent are added, stirred for 5 minutes, and then 20 parts of hydroxy acrylic resin are added, stirred for 5 minutes, and then 1 part of curing agent is added, stirred for 5 minutes, and then 12 parts of chain extender, 0.1 parts of catalyst, 0.2 parts of nano-alumina and 1 part of surfactant are added in sequence, stirred for 20 minutes, and stirred evenly to form a protective layer coating. The preparation method of INS membrane is referenced to Example 1.
[0053] Comparative Example 1
[0054] 100 parts of polycarbonate polyol resin were placed in a stirring device, and then 130 parts of solvent were added, stirred for 5 minutes, and then 30 parts of hydroxy acrylic resin were added, stirred for 5 minutes, and then 7 parts of curing agent were added, stirred for 5 minutes, and then 6 parts of chain extender, 0.5 parts of catalyst, and 0.6 parts of nano-alumina were added in sequence, stirred for 20 minutes, and stirred evenly to form a protective layer coating. The preparation method of INS membrane is referred to Example 1.
[0055] Comparative Example 2
[0056] 100 parts of polycarbonate polyol resin were placed in a stirring device, and then 130 parts of solvent were added, stirred for 5 minutes, and then 30 parts of hydroxy acrylic resin were added, stirred for 5 minutes, and then 7 parts of curing agent were added, stirred for 5 minutes, and then 6 parts of chain extender, 0.5 parts of catalyst, and 5 parts of surfactant were added in sequence, stirred for 20 minutes, and stirred evenly to form a protective layer coating. The preparation method of INS membrane is referred to Example 1.
[0057] Comparative Example 3
[0058] 100 parts of polycarbonate polyol resin were placed in a stirring device, and then 100 parts of solvent were added, stirred for 5 minutes, and then 7 parts of curing agent were added, stirred for 5 minutes, and then 6 parts of chain extender, 0.5 parts of catalyst, 0.6 parts of nano-alumina and 5 parts of surfactant were added in sequence, stirred for 20 minutes, and stirred evenly to form a protective layer coating. The preparation method of INS membrane is referred to Example 1.
[0059] Comparative Example 4
[0060] 100 parts of hydroxy acrylic resin were placed in a stirring device, and then 50 parts of solvent were added, stirred for 5 minutes, and then 7 parts of curing agent were added, stirred for 5 minutes, and then 6 parts of chain extender, 0.5 parts of catalyst, 0.6 parts of nano-alumina and 5 parts of surfactant were added in sequence, stirred for 20 minutes, and stirred evenly to form a protective layer coating. The preparation method of INS membrane is referred to Example 1.
[0061] The performance of the anti-fouling INS membrane prepared in the above examples and comparative examples was tested below:
[0062] High temperature tensile properties: According to GB / T 1040.1-2006, the experimental test was carried out at a temperature of 120°C;
[0063] Pencil hardness: Tested in accordance with GB / T 6739-1996;
[0064] Water drop angle on the membrane surface: experimental test is carried out in accordance with GB / T 30693-2014;
[0065] Coating adhesion test: Experimental test is carried out according to GB / T 9286-1998 (100-grid method);
[0066] Scratch resistance: TEBER 710 five-finger scratch tester, weight 3N, the scratch finger assembly and the test sample are placed vertically, slide back and forth 10 times, and observe whether there is any change on the diaphragm surface;
[0067] Cosmetics resistance: Apply an excessive amount of Loccitane hand cream to 50*50mm medical gauze, spread it on the surface of the part, place a 500g weight on the gauze, and then put it in an 80℃ oven. After 24 hours, observe whether there is any change on the surface of the membrane;
[0068] Sweat resistance: Soak the gauze in artificial sweat and gently wipe the membrane surface 2-3 times until the membrane surface becomes wet, then put it in an 80℃ oven and observe whether there is any change on the membrane surface after 24 hours;
[0069] Solvent resistance: Soak the gauze in ethyl ester solvent, gently wipe the surface of the membrane 2-3 times until the surface of the membrane becomes wet, then put it in an 80℃ oven, and observe whether there is any change on the surface of the membrane after 24 hours;
[0070] The main performance test results of the INS diaphragms provided by the above Examples 1-4 and Comparative Examples 1-4 are shown in the following table:
[0071]
[0072] It can be concluded from the test data of Examples 1 to 4 in the above table that the surface water drop angle of the INS diaphragm provided by the present invention reaches 108°, so that the INS diaphragm has good anti-fouling ability; and its high-temperature stretchability reaches 200%, which can meet the needs of decorating plastic products with special shapes such as irregular or large stretching or concave and convex shapes, high pencil hardness, good scratch resistance, sweat resistance and cosmetics resistance, thereby improving the life of the INS diaphragm.
[0073] Through the test data of Comparative Examples 1 to 4 in the above table, it can be concluded that in Comparative Example 4, it can be seen that the stain resistance provided by polycarbonate polyol is difficult to meet with acrylic resin; in Comparative Examples 1 and 2, in the absence of surfactants or nanopowders, the surface water drop angle fails to reach the ideal value; in Comparative Example 3, in the absence of hydroxyl acrylic resin, the adhesion to the ink layer fails to meet the requirements.
[0074] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A stain-resistant INS membrane, characterized in that: It includes a protective layer, an ink layer, an adhesive layer and a substrate layer in sequence; The protective layer is prepared by using a stain-resistant protective layer coating, and the stain-resistant protective layer coating comprises the following components in parts by weight: 80-120 parts of polycarbonate polyol resin, 20-50 parts of hydroxy acrylic resin, 2-12 parts of chain extender, 1-20 parts of curing agent, 0.1-2 parts of catalyst, 0.2-5 parts of nano powder, 1-8 parts of surfactant, 80-150 parts of solvent; The polycarbonate polyol resin is a resin prepared from polycarbonate polyol; the polycarbonate polyol includes one or more of aliphatic polycarbonate polyol, aromatic polycarbonate polyol or mixed polycarbonate polyol; The nano powder includes one or more of fumed silicon dioxide, nano alumina, nano zirconium oxide, nano zinc oxide, nano boron nitride, and titanium dioxide; The surfactant includes an organic modified silicone adjuvant.
2. The anti-fouling INS membrane according to claim 1, characterized in that: The molecular weight Mn of the polycarbonate polyol is 500-5000; and / or, The viscosity of the polycarbonate polyol resin at 25° C. is 1000-60000 cps.
3. The anti-fouling INS membrane according to claim 1, characterized in that: The solid content of the hydroxy acrylic resin is 20-60%; and / or the viscosity of the hydroxy acrylic resin at 25° C. is 500-50000 cps.
4. The anti-fouling INS membrane according to claim 1, characterized in that: The particle size of the nano powder is 2-200 nm.
5. The anti-fouling INS membrane according to any one of claims 1 to 4, characterized in that: The chain extender includes one or more of butanediol, ethylene glycol, diethylene glycol, hexanediol, glycerol, trimethylolpropane, pentaerythritol or polyether polyol; and / or, The curing agent is an isocyanate containing a rigid structure, specifically an isocyanate containing an alicyclic structure; and / or, The catalyst includes one or more of tetramethylbutylene diamine, triethylene diamine, stannous octoate, dibutyltin dilaurate, lead octoate, cobalt octoate, iron octoate, zinc naphthenate, and tetraisobutyl titanate; and / or, The solvent includes one or more of toluene, ethyl acetate, butanone, butyl ester, and N,N-dimethylformamide.
6. A method for preparing a fouling-resistant INS membrane according to any one of claims 1 to 5, characterized in that: The steps include: Putting a polycarbonate polyol resin in a stirring device, adding a solvent, a hydroxy acrylic resin, a curing agent, a chain extender, a catalyst, a nano powder and a surfactant in sequence, and stirring evenly to form a protective layer coating; coating the protective layer coating on a PET carrier film, and drying and curing to form a protective layer; In parts by weight, the added amounts of the components in the protective layer coating are: 80-120 parts of polycarbonate polyol resin, 20-50 parts of hydroxy acrylic resin, 2-12 parts of chain extender, 1-20 parts of curing agent, 0.1-2 parts of catalyst, 0.2-5 parts of nano powder, 1-8 parts of surfactant, and 80-150 parts of solvent; Printing an ink pattern on the protective layer to form an ink layer after curing; Applying adhesive on the ink layer to form an adhesive layer after curing; The protective layer, ink layer and adhesive layer form a thermal transfer film; the thermal transfer film and the substrate layer are thermally pressed together, wherein the adhesive layer of the thermal transfer film is in contact with the substrate layer; The PET carrier film is peeled off, and the protective layer and the ink layer are bonded to the surface of the substrate layer under the action of the bonding layer to form a stain-resistant INS film.
7. The method for preparing the anti-fouling INS membrane according to claim 6, characterized in that: The polycarbonate polyol resin is a resin prepared from polycarbonate polyol; the polycarbonate polyol resin includes one or more of aliphatic polycarbonate polyol, aromatic polycarbonate polyol or mixed polycarbonate polyol; The nano powder includes one or more of fumed silicon dioxide, nano alumina, nano zirconium oxide and nano boron nitride; The surfactant includes an organic modified silicone adjuvant.