A halogen-free flame-retardant cross-linked polyolefin composition and its preparation method and application

Through the application of modified layered bimetal hydroxide in polyolefin resin, the problems of unstable carbon layer and degradation of mechanical properties during the flame retardant process of polyolefin cable materials are solved, and efficient barrier effect and good mechanics are achieved. Performance, suitable for high standard cable sheathing.

CN117362805BActive Publication Date: 2024-11-12KINGFA SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311158519.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-08
Publication Date
2024-11-12
Estimated Expiration
2043-09-08

AI Technical Summary

Technical Problem

The existing halogen-free flame-retardant polyolefin cable material is unstable during the flame retardant process, which cannot effectively prevent the ignition of the cable core layer. In order to meet the low smoke, halogen-free and high flame retardant characteristics, a large amount of flame retardant is needed. , resulting in a decline in the mechanical properties of the materials.

Method used

Modified layered bimetal hydroxide as halogen-free flame retardant, and the layered bimetal hydroxide is modified by vinyl quaternary ammonium salt to increase its dispersion and layer spacing, so that it is in polyolefin resin. Form a sheet structure, participate in cross-linking reactions, and improve the carbon-forming effect and barrier ability.

Benefits of technology

The halogen-free flame-retardant crosslinked polyolefin composition has good mechanical properties and flame retardant efficiency, which can effectively prevent the ignition of the cable core layer, and the tensile strength is increased after irradiation, so that the vertical combustion carbon layer will not fall , grade V-0, suitable for rapid processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004439525300000051
    Figure BDA0004439525300000051
  • Figure BDA0004439525300000061
    Figure BDA0004439525300000061
  • Figure BDA0004439525300000062
    Figure BDA0004439525300000062
Patent Text Reader

Abstract

The present invention discloses a halogen-free flame-retardant cross-linked polyolefin composition and its preparation method and application. The halogen-free flame-retardant cross-linked polyolefin composition comprises the following components calculated by weight: 35-80 parts of polyolefin resin; 40-60 parts of modified layered double metal hydroxide; 2-4 parts of processing aid; the modified layered double metal hydroxide is obtained by modifying the layered double metal hydroxide with vinyl quaternary ammonium salt. In the present invention, the layered double metal hydroxide is modified with vinyl quaternary ammonium salt to improve the dispersibility of the layered double metal hydroxide, and double bond groups are introduced on the surface of the modified layered double metal hydroxide, which can participate in the cross-linking process of the material and can be well cross-linked without the addition of additional cross-linking agents; the interlayer spacing of the modified layered double metal hydroxide is increased, so that the polyolefin molecular chain can enter the interlayer, and the obtained polyolefin composition has good mechanical properties, flame retardant properties and processing properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of halogen-free flame retardant, and specifically relates to a halogen-free flame retardant cross-linked polyolefin composition and a preparation method and application thereof. Background Art

[0002] With the development of informatization, the country pays more and more attention to fire safety. When a fire accident occurs, cable materials play a vital role. Cable materials not only need to play a flame retardant role, but also require that they can form carbon well during the combustion process and play a certain barrier role to better prevent the internal core layer of the cable from being ignited. In order to meet higher standards, halogen-free flame-retardant polyolefin cable materials in the prior art generally need to be irradiated and cross-linked. At the same time, in order to meet the characteristics of low smoke, halogen-free and high flame retardancy, a large amount of flame retardants need to be added, which will destroy the mechanical properties of the system.

[0003] In order to improve the mechanical properties of materials in the prior art, halogen-free flame retardants are usually modified, such as aluminum hydroxide and magnesium hydroxide, to reduce their influence on the mechanical properties of the system; however, since the halogen-free flame retardants are directly decomposed to generate magnesium oxide or aluminum oxide during the flame retardant process, the carbon layer formed by physical accumulation on the surface is unstable and easily broken, and cannot play a good barrier role and effectively prevent the cable core layer from igniting. Therefore, it is necessary to provide a polyolefin composition that has both good mechanical properties and higher flame retardant efficiency. Summary of the invention

[0004] The purpose of the present invention is to overcome the technical defect that the polyolefin composition in the prior art cannot have both good mechanical properties and good charring effect, and to provide a halogen-free flame retardant cross-linked polyolefin composition, which has good charring effect, good mechanical properties and can play a barrier role, and can effectively prevent it from igniting the cable core layer.

[0005] Another object of the present invention is to provide a method for preparing the halogen-free flame retardant cross-linked polyolefin composition.

[0006] Another object of the present invention is to provide use of the halogen-free flame-retardant cross-linked polyolefin composition in preparing cable sheath materials.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A halogen-free flame-retardant cross-linked polyolefin composition comprises the following components calculated in parts by weight:

[0009] 35-80 parts of polyolefin resin;

[0010] 40-60 parts of halogen-free flame retardant;

[0011] 2 to 4 parts of processing aid;

[0012] The halogen-free flame retardant is a modified layered double metal hydroxide, and the modified layered double metal hydroxide is obtained by modifying the layered double metal hydroxide with vinyl quaternary ammonium salt.

[0013] In the present invention, polyolefin resin is selected as the base resin, and the layered double metal hydroxide is modified by using vinyl quaternary ammonium salt, so that double bonds can be introduced on the surface of the layered double metal hydroxide, the interlayer distance of the layered double metal hydroxide can be increased, and the dispersibility of the layered double metal hydroxide can be improved; when it is applied to the polyolefin resin, the peeled-off lamella structure can be well dispersed in the polyolefin resin, and effectively play a barrier role in the combustion process; at the same time, the double bonds introduced on the surface can also participate in the crosslinking process, and can be well crosslinked without the need to add an additional crosslinking agent; the modified layered double metal hydroxide has better dispersibility, can be well dispersed in the resin system, and can effectively improve the mechanical properties, so the prepared polyolefin composition has a better carbonization effect, can play a better barrier role, and effectively prevents oxygen from entering the cable material.

[0014] It should be noted that in the present invention, the layered double metal hydroxide refers to a type of hydroxide composed of two or more metal elements and having a hydrotalcite layered crystal structure or a substance obtained by intercalating such a hydroxide. In some embodiments, the layered double metal hydroxide is selected from at least one of hydrotalcite, a hydrotalcite-like compound, an anion-intercalated hydrotalcite, and an anion-intercalated hydrotalcite-like compound.

[0015] The modified layered double metal hydroxide described in the present invention can be a purchased modified layered double metal hydroxide obtained by modifying the layered double metal hydroxide with a vinyl quaternary ammonium salt, or can be prepared by oneself by referring to the prior art.

[0016] There is no particular limitation on the preparation method of the vinyl quaternary ammonium salt modified layered double metal hydroxide used as the raw material in the present invention, and any commonly used surface modification method can be used in the present invention. In some embodiments, the preparation method of the modified layered double metal hydroxide is as follows:

[0017] The layered double metal hydroxide is added into an alcohol solvent, and a dispersant is added for dispersion; vinyl quaternary ammonium salt is added for modification, and then the method is filtered and dried in sequence to obtain the method.

[0018] Specifically, the layered double metal hydroxide is added into ethanol, and a dispersant is added for ultrasonic dispersion; vinyl quaternary ammonium salt and water are then added, and the pH value of the system is adjusted to 5-6, and the mixture is fully stirred at 30-40° C. for 1.5-2.5 hours, and then filtered and dried in sequence to obtain the product.

[0019] The present invention has no special requirements on the type of dispersant, and any commercially available dispersant can be used within the range that does not impair the properties of the composition of the present invention. There is no special restriction on the amount of the dispersant used, and it is generally preferred to be 0.5wt% to 1.5wt% of the layered double metal hydroxide. In some embodiments, the dispersant is BYK-W 980 and / or NXH-1242.

[0020] Those skilled in the art may select commonly used drying conditions, such as, but not limited to, the drying temperature is 75 to 85° C., and the drying time is 7 to 9 hours.

[0021] Furthermore, the mass ratio of the layered double metal hydroxide to the vinyl silane coupling agent is not less than 10:1. It is preferably (50:1) to (25:1). It is more preferably (100:3) to (25:1), for example, it can be 26:1, 27:1, 28:1, 29:1, 30:1, 31:1, 32:1, 33:1, etc., as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention will no longer exhaustively list the specific point values ​​included in the range.

[0022] Further, the interlayer spacing of the modified layered double hydroxide is 0.22nm to 0.42nm. For example, but not limited to 0.23nm, 0.24nm, 0.25nm, 0.26nm, 0.27nm, 0.28nm, 0.29nm, 0.30nm, 0.31nm, 0.32nm, 0.33nm, 0.34nm, 0.35nm, 0.36nm, 0.37nm, 0.38nm, 0.39nm, 0.40nm, 0.41nm, 0.42nm, etc. can realize the present invention.

[0023] Furthermore, the vinyl quaternary ammonium salt is one or more of acryloyloxyethyl trimethyl ammonium chloride, acryloyloxyethyl trimethyl ammonium methyl sulfate or N,N,N-trimethyl-(1-(4-vinylphenyl))methyl ammonium salt.

[0024] It should be noted that the polyolefin resin in the present invention can be selected by a person skilled in the art from a commonly used polyolefin resin as a base resin according to the prior art. For example, but not limited to, the polyolefin resin is 10 to 15 parts of ethylene-vinyl acetate copolymer; 15 to 30 parts of metallocene linear low-density polyethylene; 5 to 20 parts of POE; and 5 to 15 parts of PE grafted maleic anhydride. Under this dosage, the mechanical properties of the obtained material are better.

[0025] Furthermore, the processing aid is an antioxidant and / or an anti-metal agent.

[0026] In the present invention, conventional antioxidants can be selected according to the prior art, including but not limited to hindered phenol antioxidants, phosphite antioxidants, diphenylamine antioxidants, copper salt antioxidants or thioether antioxidants.

[0027] Specifically, the hindered phenol antioxidant is one or more of N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide (Irganox 1098), pentaerythritol tetrakis[1093,5-di-tert-butyl-4-hydroxyphenyl)propionate (Irganox 1010), triethylene glycol bis-3-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate (Iragnox 259), β-(4-hydroxy-3,5-di-tert-butylphenyl) propionate n-octadecyl (Iragno 1076) or spiroethylene glycol bis[β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate] (ADK AO-80).

[0028] The phosphite antioxidant is one or more of 2,4-di-tert-butylphenol (Irganox 168), bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol phosphite (PEP-36) or 627A.

[0029] The diphenylamine antioxidant is 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine.

[0030] The copper salt antioxidant is a mixture of K / Cu / ZnBLEND or KI / CuI in a ratio of 8:1:1.

[0031] The thioether antioxidant is one or more of distearyl thiodipropionate, dilauryl thiodipropionate or pentaerythritol dodecapropylthioate.

[0032] In the present invention, commonly used anti-metal agents can be selected according to the prior art, such as but not limited to bis(3,5-di-tert-butyl-4-hydroxy-phenylpropionyl)hydrazine and / or 2,2-oxalyl-bis[ethyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)]propionate.

[0033] In some embodiments, the mass ratio of the hindered phenol antioxidant, the phosphite antioxidant, the thioether antioxidant and the anti-metal agent in the processing aid is (2-3): (1.5-2.5): (1.5-2.5): (0.8-1.2).

[0034] The present invention provides a method for preparing the above-mentioned halogen-free flame-retardant cross-linked polyolefin composition, comprising the following steps:

[0035] S1. The polyolefin resin, the modified layered double metal hydroxide and the processing aid are uniformly mixed to obtain a mixture;

[0036] S2. The mixture prepared in step S1 is subjected to mixing and extrusion granulation in sequence to obtain a halogen-free flame-retardant cross-linked polyolefin composition.

[0037] Furthermore, the mixing speed in step S1. is 1500-2000 rpm.

[0038] Furthermore, the temperature of the banburying in step S2 is 120-140°C.

[0039] Furthermore, the extrusion temperature in step S2. is 130-155°C.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] The invention provides a halogen-free flame-retardant cross-linked polyolefin composition. The polyolefin resin is used as a substrate. Vinyl quaternary ammonium salt is used to modify a layered double metal hydroxide, so that the dispersibility of the layered double metal hydroxide and the compatibility with the resin matrix can be effectively improved, so that the mechanical properties and processing properties of the prepared material are better; double bond groups are introduced into the surface of the modified layered double metal hydroxide, which can participate in the cross-linking process of the material and can be well cross-linked without adding an additional cross-linking agent; and the interlayer spacing of the modified layered double metal hydroxide is increased, so that intercalation and peeling are easier, and polyolefin molecular chains can be allowed to enter between layers, so that the carbonization effect of the prepared material is better and a better barrier effect can be played. The tensile strength of the prepared polyolefin composition before irradiation is greater than 13MPa, and after irradiation, cross-linking is successfully performed, and the tensile strength is improved, both of which are greater than 14MPa; the vertical combustion charcoal layer does not fall off, and the grade is V-0; when the shear rate is greater than 7000s -1 The surface of the extruded strip is still relatively smooth, which can be applied to faster processing speeds. DETAILED DESCRIPTION

[0042] The present invention is further described in detail below in conjunction with specific examples, which are only used to explain the present invention and are not used to limit the scope of the present invention. The test methods used in the following examples are conventional methods unless otherwise specified; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.

[0043] The raw materials used in each embodiment and comparative example are:

[0044] Polyolefin resin:

[0045] Ethylene-vinyl acetate copolymer (EVA): EVA 6020M, purchased from Yangzi Petrochemical-BASF Co., Ltd.;

[0046] Metallocene linear low-density polyethylene (LLDPE): LLDPE ENGAGE 3158CB, purchased from ExxonMobil;

[0047] POE elastomer: POE 58750, purchased from Dow Chemical;

[0048] PE grafted maleic anhydride: MC-218, purchased from Ningbo Nengzhiguang New Materials Technology Co., Ltd.;

[0049] Modified layered double hydroxides:

[0050] Modified layered double hydroxide 1:

[0051] Layered double hydroxide, hydrotalcite, DHT-4A, was purchased from Kyowa, Japan;

[0052] The layered double metal hydroxide is added to ethanol, and 1 wt% of the layered double metal hydroxide dispersant BYK-W 980 is added, and ultrasonic dispersion is performed; vinyl quaternary ammonium salt and water are then added, and the pH value of the mixed solution is adjusted to 5.5, and the mixture is fully stirred at 35°C for 2 hours; the mixture is filtered in turn, and dried at 80°C for 8 hours to obtain a modified layered double metal hydroxide 1; wherein the mass ratio of the layered double metal hydroxide to the vinyl quaternary ammonium salt is 100:1; and the vinyl quaternary ammonium salt is acryloyloxyethyl trimethyl ammonium chloride;

[0053] Modified layered double hydroxide 2: The same steps and parameters are used as those of modified layered double hydroxide 1, except that the mass ratio of layered double hydroxide to vinyl quaternary ammonium salt is 50:1;

[0054] Modified layered double hydroxide 3: The same steps and parameters are used as those of modified layered double hydroxide 1, except that the mass ratio of layered double hydroxide to vinyl quaternary ammonium salt is 100:3;

[0055] Modified layered double hydroxide 4: The same steps and parameters are used as those of modified layered double hydroxide 1, except that the mass ratio of layered double hydroxide to vinyl quaternary ammonium salt is 25:1;

[0056] Modified layered double metal hydroxide 5: The same steps and parameters are used as those of modified layered double metal hydroxide 1, except that the mass ratio of layered double metal hydroxide to vinyl quaternary ammonium salt is 10:1;

[0057] Modified layered double metal hydroxide 6: The same steps and parameters are used as modified layered double metal hydroxide 4, except that the vinyl quaternary ammonium salt used is acryloyloxyethyl trimethyl ammonium methyl sulfate;

[0058] Modified layered double metal hydroxide 7: The same steps and parameters are used as modified layered double metal hydroxide 4, except that the vinyl quaternary ammonium salt used is N,N,N-trimethyl-(1-(4-vinylphenyl))methylammonium salt;

[0059] Modified layered double metal hydroxide 8: The same steps and parameters as those of modified layered double metal hydroxide 4 were used, except that ammonium caprate was used;

[0060] The interlayer spacing of the modified layered double metal hydroxides 1 to 8 and the unmodified layered double metal hydroxide was tested by XRD. The test results are shown in Table 1.

[0061] Table 1 Interlayer distances of modified layered double metal hydroxides 1 to 8 and unmodified layered double metal hydroxides

[0062]

[0063]

[0064] Modified magnesium hydroxide: magnesium hydroxide, MAGNIFIN H5, purchased from Albemarle, USA; prepared by the same steps and parameters as the modified layered double hydroxide 1, except that the magnesium hydroxide is modified, and the mass ratio of magnesium hydroxide to vinyl quaternary ammonium salt is 25:1; the vinyl quaternary ammonium salt is acryloyloxyethyl trimethyl ammonium chloride;

[0065] Modified aluminum hydroxide: aluminum hydroxide, ON310S, purchased from Huber, USA; prepared according to the same steps and parameters as the modified layered double hydroxide 1, except that the aluminum hydroxide is modified, and the mass ratio of aluminum hydroxide to vinyl quaternary ammonium salt is 25:1; the vinyl quaternary ammonium salt is acryloyloxyethyl trimethyl ammonium chloride;

[0066] Processing aids:

[0067] Processing aid 1: antioxidant CHIMASSORB 944FDL, antioxidant PEP-36, antioxidant DSTDP and anti-metallic agent bis (3,5-di-tert-butyl-4-hydroxy-phenylpropionyl) hydrazine (MD-1024), all of which are commercially available, wherein their mass ratio is 2.5:2:2:1;

[0068] Processing aid 2: antioxidant CHIMASSORB 944FDL;

[0069] The parallel experiments in the embodiments and comparative examples all use the same raw materials.

[0070] Examples 1 to 10 and Comparative Examples 1 to 4

[0071] According to the formula in Tables 2 to 3, a halogen-free flame retardant cross-linked polyolefin composition was prepared according to the following preparation method:

[0072] S1. The polyolefin resin, the modified layered double metal hydroxide and the processing aid are added to a high-speed mixer in proportion and mixed at a speed of 1500 to 2000 rpm to obtain a mixture;

[0073] S2. The mixture obtained in step S1. is put into an internal mixer, and after internal mixing at 120-140° C., it is extruded and granulated at 130-155° C. by a two-stage single screw extruder to obtain a halogen-free flame-retardant cross-linked polyolefin composition.

[0074] Table 2 Amount of each component in the halogen-free flame retardant cross-linked polyolefin composition in Examples 1 to 10 (parts by weight)

[0075]

[0076]

[0077] Table 3 Amount of each component in the halogen-free flame-retardant polyolefin composition in Comparative Examples 1 to 4 (parts by weight)

[0078]

[0079] Performance Testing

[0080] 1. Test Method

[0081] The halogen-free flame-retardant cross-linked polyolefin compositions prepared in the above examples and comparative examples were subjected to performance tests:

[0082] (1) Mechanical properties test: The halogen-free flame retardant cross-linked polyolefin compositions prepared in the above embodiments and comparative examples were pressed on a flat vulcanizer at 180°C*10 min, with a pressure of 15 MPa and a sample thickness of 1 mm. After being placed at room temperature for 16 h, the mechanical properties of the 1 mm thick sample before irradiation were measured with reference to standard GB / T 1040.2-2018, and the mechanical properties were tested after irradiation with an irradiation dose of 5 Mard using the same method and standard.

[0083] (2) Flame retardant performance test: The halogen-free flame retardant cross-linked polyolefin composition prepared in the above examples and comparative examples was pressed on a flat vulcanizer at 180°C*10min, with a pressure of 15MPa and a sample thickness of 3mm. After being placed at room temperature for 16h, the vertical combustion test was conducted according to the UL 94-2018 standard. The combustion grades were V-0, V-1, V-2 and NR (no grade) in sequence, and the flame retardant performance and charring performance decreased in sequence. It was also observed whether the char layer fell off, and if it fell off, it indicated that the charring was poor.

[0084] (3) Processing performance: 100 g of each of the halogen-free flame-retardant cross-linked polyolefin compositions prepared in the above examples and comparative examples were dried in an oven at 120° C. for 30 min. A high pressure capillary rheometer was used for testing. -1 , 5000s -1 , 7000s -1 Different shear rates, observe the appearance of the extruded strips at different shear rates, and divide them into smooth and rough. Note the shear rate when the extruded strips are smooth; the smoother the extruded strips, the better the processing performance, that is, it can meet the faster extrusion processing speed.

[0085] 2. Test results

[0086] Table 4 Performance test results of various embodiments and comparative examples

[0087]

[0088]

[0089] It can be seen from Table 4 that the halogen-free flame-retardant cross-linked polyolefin composition prepared by the present invention has good mechanical properties and flame retardant properties, wherein the tensile strength before irradiation is greater than 13MPa, and after irradiation, the cross-linking is successful, and the tensile strength is improved, both greater than 14MPa; the vertical combustion charcoal layer does not fall off, and the grade is V-0; when the shear rate is greater than 7000s -1 The surface of the extruded strip is still relatively smooth, which can be applied to faster processing speeds.

[0090] It can be seen from Examples 1 to 5 that when the mass ratio of the layered double metal hydroxide to the vinyl silane coupling agent is in the range of (100:3) to (25:1), the comprehensive performance of the halogen-free flame retardant cross-linked polyolefin composition obtained is better, and the mechanical properties of the obtained material are further improved when the flame retardant effect and processing performance are equivalent.

[0091] It can be seen from Comparative Example 1 that when unmodified layered double metal hydroxide is used, the obtained halogen-free flame retardant cross-linked polyolefin composition has poor compatibility, fails to be peeled and dispersed, and the mechanical properties, carbon layer strength, and processing properties of the obtained material are significantly reduced;

[0092] It can be seen from Comparative Example 2 that when the layered double hydroxide is modified with an alkyl ammonium salt, the obtained halogen-free flame-retardant cross-linked polyolefin composition cannot be cross-linked by irradiation because its surface does not contain double bonds; instead, the tensile strength decreases after irradiation, and the flame retardant properties of the material decrease;

[0093] It can be seen from Comparative Examples 3 and 4 that the flame retardant properties and processing properties of the halogen-free flame retardant cross-linked polyolefin composition prepared by modifying magnesium hydroxide or aluminum hydroxide with vinyl ammonium salt are significantly reduced.

[0094] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A halogen-free flame-retardant cross-linked polyolefin composition, characterized in that: The composition comprises the following components calculated by weight: 35-80 parts of polyolefin resin; 40-60 parts of halogen-free flame retardant; 2 to 4 parts of processing aid; The halogen-free flame retardant is a modified layered double metal hydroxide, and the modified layered double metal hydroxide is obtained by modifying the layered double metal hydroxide with a vinyl quaternary ammonium salt; The mass ratio of the layered double metal hydroxide to the vinyl quaternary ammonium salt is (10:1) to (100:1); the layered double metal hydroxide is hydrotalcite; The polyolefin resin comprises 10 to 15 parts of ethylene-vinyl acetate copolymer, 15 to 30 parts of metallocene linear low-density polyethylene, 5 to 20 parts of POE, and 5 to 15 parts of PE grafted maleic anhydride.

2. The halogen-free flame-retardant cross-linked polyolefin composition according to claim 1, characterized in that: The mass ratio of the layered double metal hydroxide to the vinyl quaternary ammonium salt is (25:1) to (50:1).

3. The halogen-free flame-retardant cross-linked polyolefin composition according to claim 1, characterized in that: The interlayer distance of the modified layered double metal hydroxide is 0.22nm to 0.42nm.

4. The halogen-free flame-retardant cross-linked polyolefin composition according to claim 1, characterized in that: The vinyl quaternary ammonium salt is one or more of acryloyloxyethyl trimethyl ammonium chloride, acryloyloxyethyl trimethyl ammonium methyl sulfate or N,N,N-trimethyl-(1-(4-vinylphenyl))methyl ammonium salt.

5. The halogen-free flame-retardant cross-linked polyolefin composition according to claim 1, characterized in that: The preparation method of the modified layered double metal hydroxide is as follows: The layered double metal hydroxide is added into an alcohol solvent, and a dispersant is added for dispersion; vinyl quaternary ammonium salt is added for modification, and then the method is filtered and dried in sequence to obtain the method.

6. The halogen-free flame-retardant cross-linked polyolefin composition according to claim 1, characterized in that: The processing aid is an antioxidant and / or an anti-metal agent.

7. The method for preparing the halogen-free flame-retardant cross-linked polyolefin composition according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. The polyolefin resin, the modified layered double metal hydroxide and the processing aid are mixed to obtain a mixture; S2. The mixture prepared in step S1 is subjected to mixing and extrusion granulation in sequence to obtain a halogen-free flame-retardant cross-linked polyolefin composition.

8. Use of the halogen-free flame-retardant cross-linked polyolefin composition according to any one of claims 1 to 6 in the preparation of cable sheath materials.