A preparation process and application of high-toughness and high-filling PP sheet

By adding fillers and elastomers such as modified heavy calcium carbonate and nano-calcium carbonate to PP sheets, combined with the high-mixer process, the problems of insufficient performance and poor environmental protection of PP sheets in low-temperature environments have been solved, and highly filled PP has been realized. The board has high toughness, good dimensional stability and environmental protection.

CN117362832BActive Publication Date: 2024-10-01浙江海象新材料股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311439722.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-01
Publication Date
2024-10-01
Estimated Expiration
2043-11-01

AI Technical Summary

Technical Problem

Existing PP boards have poor performance in low-temperature environments, low impact strength, poor toughness, poor aging resistance and dimensional stability, and commonly used PVC materials are not environmentally friendly and difficult to biodegrade.

Method used

Highly filled PP sheet preparation process is adopted, including PP, linear low density polyethylene, modified heavy calcium carbonate, nano calcium carbonate, polyolefin elastomer, coupling agent, lubricant, antioxidant, glass fiber, and hyperbranched epoxy Resin and silicone epoxy modified acrylic resin are extruded through the preparation method of modified heavy calcium carbonate and a high mixer to fully mix them to improve the mechanical properties and dimensional stability of the board.

Benefits of technology

It improves the bending, tensile strength, hardness, waterproof performance and environmental protection of PP sheets, enhances the mechanical properties and dimensional stability of the sheets, extends the service life, promotes the recycling of waste plastics, and alleviates environmental pollution problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004525639950000161
    Figure BDA0004525639950000161
  • Figure BDA0004525639950000171
    Figure BDA0004525639950000171
  • Figure BDA0004525639950000181
    Figure BDA0004525639950000181
Patent Text Reader

Abstract

The present invention relates to a preparation process and application of a high-toughness and high-filling PP sheet. The high-toughness and high-filling PP sheet comprises the following components, in parts by weight: 30-40 parts of PP, 1-10 parts of linear low-density polyethylene, 20-40 parts of modified heavy calcium carbonate, 8-15 parts of nano calcium carbonate, 1-3 parts of polyolefin elastomer, 0.1-1 part of coupling agent, 0.1-2 parts of lubricant, 0.1-1 part of antioxidant, 10-20 parts of glass fiber, 0.1-3 parts of light stabilizer, 2-5 parts of hyperbranched epoxy resin, and 0.1-1 part of silicone epoxy modified acrylic resin. The components of the present invention have synergistic effects and good compatibility. The prepared high-toughness and high-filling PP sheet has excellent comprehensive performance, and has many advantages such as non-toxic and tasteless, low water absorption, dimensional stability, heat resistance, friction resistance, corrosion resistance, shrinkage resistance, strong impact resistance, and not easy to deform.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of composite material preparation, and specifically relates to a preparation process of a high-toughness and high-filling PP plate. Background Art

[0002] Polypropylene, referred to as PP, is a thermoplastic resin made by propylene polymerization. PP sheet is a plastic sheet made by adding various functional additives to PP resin through extrusion, calendering, cooling, cutting and other processes. PP sheet is odorless, non-toxic, tasteless and meets national health standards; it has a low density and is the lightest of general-purpose plastics. It can be used for a long time at 100°C without deformation. It also has excellent electrical insulation properties and chemical stability, and almost does not absorb water. It does not react with most chemicals. At present, PP sheet has been widely used in various fields of packaging and daily life such as industry, agriculture, medical treatment, and health. It is the largest and fastest growing type of polymer material in the world. This is mainly due to its multiple sources of raw materials, low price, excellent material properties, good electrical insulation and chemical stability, and easy processing and molding.

[0003] Although PP has many advantages, it also has its shortcomings: 1. Due to the poor performance of PP in low temperature environment, there is a problem of crystallization during blistering, which leads to uneven molding in all directions, poor plasticity, and difficulty in blistering. 2. Poor low temperature resistance, brittle in low temperature environment. 3. Since PP is a crystalline polymer, there are large spherulites inside, resulting in low impact strength and poor toughness of PP. 4. Poor aging resistance, large molding shrinkage, easy to burn, and due to its non-polar characteristics, it has poor compatibility with other polar polymers and inorganic fillers, thus limiting its application as a raw material or special material for injection molding, fiber, film and other products. 5. The surface hardness of PP resin itself is not enough to cope with long-term friction, damage, etc. At present, the most commonly used method is to enhance, fill, alloy, etc. of PP, but even so, the wear resistance and puncture resistance of PP sheets are still unsatisfactory.

[0004] CN115124793A discloses a highly filled SPC sheet and its preparation process and application, wherein the raw materials include the following components: PVC, calcium powder, polyester hyperbranched polymer dispersant, calcium zinc stabilizer, CPE, ACR, internal lubricant, external lubricant, and pigment. The SPC sheet of the present invention has a high calcium powder addition amount. It has a wide temperature adaptability range, good flatness and dimensional stability, high mechanical strength, high and low temperature resistance, shrinkage and warping resistance, and good waterproof performance. However, PVC sheets have the disadvantage of poor environmental protection, such as the generation of toxic hydrogen chloride and carbon monoxide gas by cracking, and the generation of toxic gases such as dioxins after combustion. In addition, the dimensional stability of PVC floors is not good, and the floors are not classified and recycled. After being abandoned and buried, they cannot be biodegraded, causing white pollution.

[0005] CN107603028A discloses a rubber calcium carbonate modified PP foaming sheet, the raw materials include bulk PP, copolymerized PP, linear low-density polyethylene, ethylene-vinyl acetate copolymer, additives, and modified natural rubber. The additives include a foaming agent, a crosslinking agent, a foaming initiator, and a toughening agent, and the toughening agent is a mixture of natural rubber and nano calcium carbonate. However, zinc oxide, one of the foaming agent blends in the raw materials, can cause systemic allergic reactions in some people who are allergic to it.

[0006] CN113150466A discloses an SPC floor, the raw materials of which include PVC resin, heavy calcium carbonate powder, nano calcium carbonate, lubricant, calcium zinc stabilizer, microcrystalline cellulose, superdispersant, tourmaline powder, carbon nanotubes, and antibacterial agent. The floor of the invention has good tensile strength, stability, antibacterial property, lower dimensional deformation rate, etc., but PVC material is used in the raw materials, which is not as safe as PP material. In the preparation process, calcium zinc stabilizer needs to be added additionally, and the addition of calcium zinc stabilizer will lead to a decrease in the softening point of the board.

[0007] CN111320816A discloses a PP floor and a preparation method thereof, wherein the raw materials include polypropylene, filler, polyolefin elastomer, and coupling agent. The polypropylene floor provided by the invention has the advantages of being non-toxic, tasteless, and having good dimensional stability, but the board strength is not high and the water absorption resistance is not excellent. Summary of the invention

[0008] The present invention provides the following technical solutions:

[0009] The invention provides a high-toughness and high-filling PP plate, which comprises the following components in parts by weight: 30-40 parts of PP, 1-10 parts of linear low-density polyethylene, 20-40 parts of modified heavy calcium carbonate, 8-15 parts of nano calcium carbonate, 1-3 parts of polyolefin elastomer, 0.1-1 part of coupling agent, 0.1-2 parts of lubricant, 0.1-1 part of antioxidant, 10-20 parts of glass fiber, 0.1-3 parts of light stabilizer, 2-5 parts of hyperbranched epoxy resin and 0.1-1 part of silicone epoxy modified acrylic resin.

[0010] The preparation method of the modified heavy calcium carbonate:

[0011] (1) Weigh 20-30 g of heavy calcium carbonate, add 50-100 mL of water and anhydrous ethanol, the volume ratio of water to anhydrous ethanol is 1:3, then stir evenly to form a suspension, and then heat the suspension;

[0012] (2) When the temperature reaches 60-70° C., add 10-20 g of sodium stearate to the heavy calcium carbonate suspension and stir to react for 40-50 min;

[0013] (3) After the reaction is completed, the product is repeatedly washed with water and anhydrous ethanol for multiple times, filtered and separated, and vacuum dried at 50-60° C. for 24-30 hours to obtain modified heavy calcium carbonate.

[0014] Preferably, the particle size of the heavy calcium carbonate is 325-800 mesh; more preferably, the particle size of the heavy calcium carbonate is 400 mesh.

[0015] Preferably, the average particle size of the nano-calcium carbonate is 10 to 30 nm; more preferably, the average particle size of the nano-calcium carbonate is 20 nm.

[0016] Preferably, the polyolefin elastomer is at least one of ethylene-octene copolymer and ethylene-propylene copolymer; more preferably, the polyolefin elastomer is ethylene-octene copolymer.

[0017] Preferably, the coupling agent is at least one of a titanate coupling agent, an aluminate coupling agent, and a silane coupling agent; more preferably, the coupling agent is a titanate coupling agent TCA-K 12.

[0018] Preferably, the lubricant is at least one of stearic acid, paraffin, PE wax, stearate, monoglyceride, PETS, EBS, and TAF lubricants; more preferably, the lubricant is PE wax.

[0019] Preferably, the antioxidant is at least one of antioxidant 1010 and antioxidant 168; more preferably, the antioxidant is antioxidant 168.

[0020] Preferably, the diameter of the glass fiber monofilament is 11-17 μm, and the particle size is 10-350 μm; more preferably, the diameter of the glass fiber is 13 μm, and the length is 100 μm.

[0021] Preferably, the light stabilizer is at least one of zinc phosphate, benzotriazole, acrylic acid, and triazines; more preferably, the light stabilizer is benzotriazole.

[0022] The present invention also discloses a preparation process of the high-toughness and high-filling PP sheet:

[0023] The steps are as follows:

[0024] (1) Add 30-40 parts of PP, 1-10 parts of linear low-density polyethylene, 20-40 parts of modified heavy calcium carbonate, 8-15 parts of nano calcium carbonate, 1-3 parts of polyolefin elastomer, 0.1-1 part of coupling agent, 0.1-2 parts of lubricant, 0.1-1 part of antioxidant, 10-20 parts of glass fiber, 0.1-3 parts of light stabilizer, 2-5 parts of hyperbranched epoxy resin, and 0.1-1 part of silicone epoxy modified acrylic resin into a high mixer and mix thoroughly to obtain a uniform mixture at a mixing temperature of 90-120° C. for 8-15 min;

[0025] (2) After heating to 110-120°C, move to a cold mixer and cool the material to 40-60°C;

[0026] (3) The cooled mixed material of step (2) is heated and extruded through an extruder, and then passes through a sheet die for extrusion molding, and the molded sheet is extruded and shaped through a calender.

[0027] In step (3), the speed of the extruder and the screw is 150-250 r / min, the head temperature is 150-200° C., the main body temperature of the extruder is 190-230° C., and the extrusion pressure is 5-8 MPa.

[0028] The present application uses the high-toughness and high-filling PP board prepared by the above method in the production of flooring.

[0029] Beneficial effects of the present invention:

[0030] 1. The present invention adopts modified heavy calcium carbonate and polypropylene to prepare a composite material, and the composite material has high bending and tensile strength, high hardness, is environmentally friendly and pollution-free, and prevents water absorption.

[0031] 2. The present invention adds linear low-density polyethylene, nano-calcium carbonate, glass fiber, hyperbranched epoxy resin, polyolefin elastomer, silicone epoxy-modified acrylic resin, and modified calcium carbonate to a polypropylene composite material. Due to the synergistic effect of these substances and the introduction of hyperbranched epoxy resin, they have a higher addition amount and dispersibility in the polypropylene composite material, and the prepared PP sheet has good waterproof performance, mechanical strength, dimensional stability, etc.

[0032] 3. At the same time, the present invention has a positive effect on the recycling of waste plastics such as polypropylene, which is helpful to alleviate environmental pollution problems to a certain extent, that is, it solves the shortage of resources and turns waste into treasure.

[0033] The functions of the raw materials in the present invention are specifically described as follows:

[0034] Polypropylene: A thermoplastic synthetic resin with excellent performance. It is a colorless, translucent, thermoplastic, lightweight general-purpose plastic with chemical resistance, heat resistance, electrical insulation, high-strength mechanical properties and good high-wear processing performance. It is widely used in the production of clothing, blankets and other fiber products, medical equipment, automobiles, bicycles, parts, conveying pipelines, chemical containers, etc., and is also used in food and drug packaging.

[0035] Linear low-density polyethylene: LLDPE for short in English, is a linear ethylene main chain formed by copolymerization of ethylene and a small amount of α-olefin with very short comonomer side chains. Linear low-density polyethylene is a non-toxic, tasteless, odorless milky white particle with a density of 0.918-0.935 g / cm 3 . Compared with LDPE, it has higher softening temperature and melting temperature, and has advantages such as high strength, good toughness, high rigidity, good heat resistance and cold resistance. It also has good environmental stress cracking resistance, impact strength, tear strength and other properties, and can resist acids, alkalis, organic solvents, etc. and is widely used in industries, agriculture, medicine, health and daily necessities. Linear low-density polyethylene (LLDPE) resin is called the third generation of polyethylene. In addition to the properties of general polyolefin resins, its tensile strength, tear strength, environmental stress cracking resistance, low temperature resistance, heat resistance and puncture resistance are particularly superior. As a linear PE, LLDPE has a narrow molecular weight distribution, a flexible molecular chain, good crystallinity, environmental stress cracking resistance, and impact resistance. Therefore, it can be used in PP materials to improve properties such as toughness and elongation. However, POE and LLDPE have a good improvement in toughness for PP filling materials, but the strength will be reduced. The simultaneous use of POE and LLDPE has a good synergistic toughening effect, and the strength reduction is small.

[0036] Modified heavy calcium carbonate: Adding a small amount of inorganic filler can act as a nucleating agent, refine the grains, and improve the crystallinity of polypropylene, thereby improving the mechanical properties of polypropylene and improving the balance of polypropylene materials. The added inorganic filler can increase the heat deformation temperature of polypropylene sheet materials, increase the dimensional stability of products, reduce molding shrinkage, increase rigidity, increase the impact strength of polypropylene sheet materials and improve impact resistance. In addition, inorganic fillers also have the function of melt flow promoters. The inorganic filler can enhance the mechanical properties of PP through twin-screw extrusion mixing and pelletizing. The interfacial adhesion between the filler and the polymer greatly affects the mechanical properties of the composite material. Nano calcium carbonate and modified heavy calcium carbonate have a reinforcing effect on POE cross-linked elastomers as reinforcing agents.

[0037] Polyolefin elastomer: POE for short. POE, as a toughening agent and heterogeneous nucleating agent, destroys the integrity of PP spherulites, refines the PP particle size, and significantly reduces the average particle size of spherulites, which has a good toughening effect on PP. After adding the toughening agent POE, PP changes from brittle fracture to tough fracture. POE has a good processing morphology and good compatibility with PP. Under good shear force, it is easy to obtain a smaller dispersed particle size and a narrower particle size distribution in the PP matrix, so it has a significant toughening effect on PP materials. Nano calcium carbonate and modified heavy calcium carbonate have a reinforcing effect on POE cross-linked elastomer as reinforcing agents. Because POE has a small cohesive energy and high shear sensitivity, it has good compatibility with PP during processing. POE as a toughening agent to toughen PP can obtain a smaller dispersed phase particle size and a narrower particle size distribution; especially for inorganic filled PP systems, POE can also improve the dispersibility of fillers. POE forms a uniform sea-island structure in the PP continuous phase. Since the viscosity of POE and PP is similar, a finer dispersed phase can be formed. By inducing a large number of silver streaks in the PP phase, the room temperature and low temperature impact strength of PP is effectively improved, and POE has a significant slow-down effect on the yield strength of PP. Studies have shown that LDPE blended with PP can obtain higher elongation at break and better elasticity.

[0038] Coupling agent TCA-K 12: A plastic additive that improves the interfacial properties of synthetic resin and modified heavy calcium carbonate or reinforcing materials in plastic compounding, also known as a surface modifier. It can reduce the viscosity of synthetic resin melt during plastic processing, improve the dispersion of fillers to improve processing performance, and thus enable the product to obtain good surface quality and mechanical, thermal and electrical properties. At the same time, when the coupling agent is a titanate coupling agent, especially TCA-K 12, the dimensional stability of the board is excellent. As the particle size increases or decreases, the dimensional stability of the wood board will decrease. It is speculated that the possible reason is that during the preparation of the wood board, the modified heavy calcium carbonate of 325 to 800 mesh can be well dispersed in the system, and at the same time, the TCA-K 12 type titanate coupling agent ensures that the modified heavy calcium carbonate is evenly wrapped in the middle by polypropylene, the force is evenly dispersed, and the dimensional stability of the wood board is ensured.

[0039] Lubricant PE wax: The lubricant in the formula can increase the material performance, improve the extrusion speed and the appearance quality of the sheet. Composite lubricant is an additive that can improve the composite processing performance of materials. According to its mechanism of action, it can be divided into external lubricants and internal lubricants. External lubricants can increase the lubricity of the material surface during processing. Internal lubricants can reduce the internal friction of polymers, increase the melting rate and melt deformation of plastics, reduce melt viscosity and improve plasticization performance. In fact, each lubricant has a role in achieving a certain requirement. It is always the joint effect of internal and external lubrication, but it is more prominent in one aspect. The same lubricant will show different lubricating effects in different polymers or under different processing conditions. For example, under high temperature and high pressure, the internal lubricant will be squeezed out and become an external lubricant. Lubricants are also often used in plastic processing to improve fluidity and demoulding properties, and prevent adhesion in the machine or mold to produce defects such as fish eyes.

[0040] Antioxidant 168: Adding antioxidants to PP sheets can play an antioxidant role, thereby extending its service life. Antioxidants can prevent PP sheets from undergoing oxidation reactions under the influence of factors such as ultraviolet rays, oxygen and moisture, thereby reducing their strength and performance. There are many types of antioxidants, and commonly used ones include phosphites, thio compounds, etc. The antioxidant 168 used in the present invention belongs to the phosphite antioxidant class. Phosphites have a good effect. They can be embedded in the molecular chain of PP sheets to prevent the occurrence of oxidation reactions.

[0041] Glass fiber: In the present invention, glass fiber can improve the disadvantage of the decrease in tensile and flexural strength of mechanical properties caused by the addition of linear low-density polyethylene to PP. The increase of glass fiber increases the tensile strength, flexural strength and modulus of PP / LLDPE copolymer.

[0042] Light stabilizer benzotriazole: It is an additive for polymer products (such as plastics, rubber, coatings, synthetic fibers). It can shield or absorb the energy of ultraviolet rays, quench singlet oxygen, and decompose hydroperoxides into inactive substances. It can eliminate or slow down the possibility of photochemical reactions under the radiation of light, prevent or delay the process of photoaging, and thus achieve the purpose of extending the service life of polymer products. Ultraviolet rays in sunlight are the main cause of aging effects on polymer materials. Although ultraviolet rays only account for about 5% of sunlight, they have great energy. After absorbing ultraviolet rays, polymer products are sufficient to cause self-oxidation and degradation of polymers, destroy the chemical bonds of polymers, break them, and cross-link them, resulting in the deterioration of the appearance and physical and mechanical properties of polymer products such as color, reduced strength, and shortened life. This process is called photoredox or photoaging. Light stabilizers have different functions due to their own structures and varieties. Some can shield, reflect or absorb ultraviolet rays and convert them into harmless heat energy; some can quench the excited state of molecules or groups excited by ultraviolet rays, returning them to the ground state, eliminating or slowing down the possibility of photo-oxidation-reduction reactions; some can capture free radicals generated by photo-oxidation-reduction, thereby preventing free radical reactions that cause product aging and protecting products from ultraviolet damage. Light stabilizers can be divided into the following categories according to their mechanism of action: (1) light shielding agents (2) ultraviolet absorbers (3) quenchers (4) free radical scavengers (5) hydroperoxide decomposers. The light stabilizer used in the present invention is a benzotriazole, specifically benzotriazole. It can effectively absorb ultraviolet rays with a wavelength of 290 to 410 nm, but rarely absorbs visible light, and it itself has good thermal stability and light stability. It is used together with a hindered light stabilizer as an auxiliary light stabilizer, especially in polyolefins or coatings.

[0043] Hyperbranched epoxy resin: Hyperbranched epoxy resin can increase the dispersibility and stability of inorganic materials in the resin, thereby increasing the filling amount of inorganic materials in the resin. Because the hyperbranched polymer itself has a certain rigidity, while using the performance characteristics of the holes inside to increase toughness, it can also greatly improve the strength of the composite material. Therefore, in the present invention, the hyperbranched epoxy resin can well bond PP and various additives.

[0044] Silicone epoxy modified acrylic resin: Silicone epoxy modified acrylic resin dispersion has better performance than acrylic copolymers, and improves the stain resistance and hydrophobicity of high-filled PP sheets. The reason is that silicone is a low surface energy material. The low surface tension and hydrophobicity and oleophobicity of its main chain siloxane give it excellent stain resistance. The compounding of silicone with water-based acrylic resin can effectively improve the water resistance and stain resistance of water-based acrylic coating. Introducing silicone into organic synthetic resin can make the performance of silicone and organic synthetic resin more perfect. Acrylic resin has excellent adhesion, good mechanical properties, chemical stability, and abundant raw material sources and low cost. The Si-O bond energy in silicone compounds is much greater than the CC bond energy and CO bond energy, so it has low glass transition temperature, excellent high temperature resistance, oxidative degradation resistance, weather resistance, excellent hydrophobicity, light retention, impact resistance, abrasion resistance and UV resistance. Grafting polysiloxane with acrylate can significantly reduce the surface tension, water absorption, and staining of polyacrylate, and improve its resistance to high and low temperatures. DETAILED DESCRIPTION

[0045] In order to further understand the present invention, a preparation process of a high-toughness and high-filling PP plate provided by the present invention is described in detail below in conjunction with embodiments.

[0046] In the following statements:

[0047] Polypropylene: Model: J-150H, source: Lotte Chemical.

[0048] Linear low-density polyethylene: Model: DNDA 8320, source: Sinopec Fujian Refining.

[0049] Heavy calcium carbonate: 400 mesh.

[0050] Nano calcium carbonate: The particle size of nano calcium carbonate is 20nm.

[0051] Polyolefin elastomer: Model: XLT 8677, source: Shenzhen Wansuyuan Rubber & Plastic Co., Ltd.

[0052] Titanate coupling agent: Model TCA-K12, source: Nanjing Nengde New Materials Technology Co., Ltd.

[0053] PE wax: Model is PE-110, source: Ningbo Beitian Chemical Co., Ltd.

[0054] Antioxidant 168: CAS number: 31570-04-4, source: Tianjin Lianlong New Materials Co., Ltd.

[0055] Glass fiber: Glass fiber type: alkali-free; mesh number: 80; single fiber diameter: 13μm; particle size: 100μm, source: Wuhe Weijia Composite Materials Co., Ltd.

[0056] Hyperbranched epoxy resin: Model HyPer E 102, yellow transparent liquid, epoxy value 0.15±0.05mol / 100g, molecular weight 3200-3600, source: Wuhan Hyperbranched Resin Technology Co., Ltd.

[0057] Silicone epoxy modified acrylate: Model: SJ-804, from Jining Tangyi Chemical Co., Ltd.

[0058] Acrylate copolymer: Product number: GY63977-500g, source: Shanghai Hansi Chemical Co., Ltd.

[0059] Epoxy acrylate: Model: EBECRYL 600, molecular weight 500, viscosity 3000mPa.s (60℃), source: Shanghai Kaiyin Chemical Co., Ltd.

[0060] Polyurethane acrylate: Model: EBECRYL 9260, molecular weight 1500, viscosity 3000mPa.s (60℃), source: Shanghai Kaiyin Chemical Co., Ltd.

[0061] Hyperbranched polyamide resin: Model HyPer HPN 202, source: Wuhan Hyperbranched Resin Technology Co., Ltd.

[0062] Embodiment 1:

[0063] A high-toughness and high-filling PP sheet preparation process comprises the following steps:

[0064] (1) 32.5 g of PP, 5.0 g of linear low-density polyethylene, 30 g of modified heavy calcium carbonate, 10.0 g of nano calcium carbonate, 2.0 g of polyolefin elastomer, 0.5 g of titanate coupling agent TCA-K12, 1 g of PE wax, 0.5 g of antioxidant 168, 10.0 g of glass fiber, 1.0 g of benzotriazole, 3 g of hyperbranched epoxy resin, and 0.5 g of silicone epoxy modified acrylic resin were added into a high mixer and mixed thoroughly to obtain a uniform mixture at a mixing temperature of 110° C. for 11 min.

[0065] (2) After heating to 115°C, move to a cold mixer and cool the material to 45°C;

[0066] (3) The cooled mixed material of step (2) is heated and extruded through an extruder, and then passes through a sheet die for extrusion molding, and the molded sheet is extruded and shaped through a calender.

[0067] In step (3), the speed of the extruder feeder is the same as the screw speed, both of which are 180 r / min, the die temperature is 170° C., the extruder main engine temperature is 210° C., and the extrusion pressure is 7 MPa.

[0068] The preparation method of the modified heavy calcium carbonate is:

[0069] (1) Weigh 30 g of heavy calcium carbonate, add 100 mL of water and anhydrous ethanol, the volume ratio of water to anhydrous ethanol is 1:3, then stir evenly to form a suspension, and then heat the suspension;

[0070] (2) After the above is heated to 70°C, add 20g of sodium stearate and stir to react for 50min;

[0071] (3) After the reaction is completed, the product is repeatedly washed with water and anhydrous ethanol for multiple times, separated by suction filtration, and vacuum dried at 60° C. for 30 h to obtain modified heavy calcium carbonate.

[0072] Comparative Example 1:

[0073] A high-toughness and high-filling PP sheet preparation process comprises the following steps:

[0074] (1) 32.5 g of PP, 5.0 g of linear low-density polyethylene, 30 g of modified heavy calcium carbonate, 10.0 g of nano calcium carbonate, 2.0 g of polyolefin elastomer, 0.5 g of titanate coupling agent TCA-K12, 1 g of PE wax, 0.5 g of antioxidant 168, 10.0 g of glass fiber, 1.0 g of benzotriazole, 3 g of hyperbranched epoxy resin, and 0.5 g of acrylic copolymer were added into a high-speed mixer and mixed thoroughly to obtain a uniform mixture at a mixing temperature of 110° C. for 11 min.

[0075] (2) After heating to 115°C, move to a cold mixer and cool the material to 45°C;

[0076] (3) The cooled mixed material of step (2) is heated and extruded through an extruder, and then passes through a sheet die for extrusion molding, and the molded sheet is extruded and shaped through a calender.

[0077] In step (3), the speed of the extruder feeder is the same as the screw speed, both of which are 180 r / min, the die temperature is 170° C., the extruder main engine temperature is 210° C., and the extrusion pressure is 7 MPa.

[0078] The preparation method of the modified heavy calcium carbonate is the same as that in Example 1 and will not be repeated here.

[0079] Comparative Example 2:

[0080] A high-toughness and high-filling PP sheet preparation process comprises the following steps:

[0081] (1) 32.5 g of PP, 5.0 g of linear low-density polyethylene, 30 g of modified heavy calcium carbonate, 10.0 g of nano calcium carbonate, 2.0 g of polyolefin elastomer, 0.5 g of titanate coupling agent TCA-K12, 1 g of PE wax, 0.5 g of antioxidant 168, 10.0 g of glass fiber, 1.0 g of benzotriazole, 3 g of hyperbranched epoxy resin, and 0.5 g of epoxy acrylate were added into a high-speed mixer and mixed thoroughly to obtain a uniform mixture at a mixing temperature of 110° C. for 11 min.

[0082] (2) After heating to 115°C, move to a cold mixer and cool the material to 45°C;

[0083] (3) The cooled mixed material of step (2) is heated and extruded through an extruder, and then passes through a sheet die for extrusion molding, and the molded sheet is extruded and shaped through a calender.

[0084] In step (3), the speed of the extruder feeder is the same as the screw speed, both of which are 180 r / min, the die temperature is 170° C., the extruder main engine temperature is 210° C., and the extrusion pressure is 7 MPa.

[0085] The preparation method of the modified heavy calcium carbonate is the same as that in Example 1 and will not be repeated here.

[0086] Comparative Example 3:

[0087] A high-toughness and high-filling PP sheet preparation process comprises the following steps:

[0088] (1) 32.5 g of PP, 5.0 g of linear low-density polyethylene, 30 g of modified heavy calcium carbonate, 10.0 g of nano calcium carbonate, 2.0 g of polyolefin elastomer, 0.5 g of titanate coupling agent TCA-K12, 1 g of PE wax, 0.5 g of antioxidant 168, 10.0 g of glass fiber, 1.0 g of benzotriazole, 3 g of hyperbranched epoxy resin, and 0.5 g of polyurethane acrylate were added into a high-speed mixer and mixed thoroughly to obtain a uniform mixture at a mixing temperature of 110° C. for 11 min.

[0089] (2) After heating to 115°C, move to a cold mixer and cool the material to 45°C;

[0090] (3) The cooled mixed material of step (2) is heated and extruded through an extruder, and then passes through a sheet die for extrusion molding, and the molded sheet is extruded and shaped through a calender.

[0091] In step (3), the speed of the extruder feeder is the same as the screw speed, both of which are 180 r / min, the die temperature is 170° C., the extruder main engine temperature is 210° C., and the extrusion pressure is 7 MPa.

[0092] The preparation method of the modified heavy calcium carbonate is the same as that in Example 1 and will not be repeated here.

[0093] Comparative Example 4:

[0094] A high-toughness and high-filling PP sheet preparation process comprises the following steps:

[0095] (1) 37.5 g of PP, 30 g of modified heavy calcium carbonate, 10.0 g of nano calcium carbonate, 2.0 g of polyolefin elastomer, 0.5 g of titanate coupling agent TCA-K12, 1 g of PE wax, 0.5 g of antioxidant 168, 10.0 g of glass fiber, 1.0 g of benzotriazole, 3 g of hyperbranched epoxy resin, and 0.5 g of silicone epoxy modified acrylic resin were added into a high mixer and mixed thoroughly to obtain a uniform mixture at a mixing temperature of 110° C. for 11 min.

[0096] (2) After heating to 115°C, move to a cold mixer and cool the material to 45°C;

[0097] (3) The cooled mixed material of step (2) is heated and extruded through an extruder, and then passes through a sheet die for extrusion molding, and the molded sheet is extruded and shaped through a calender.

[0098] In step (3), the speed of the extruder feeder is the same as the screw speed, both of which are 180 r / min, the die temperature is 170° C., the extruder main engine temperature is 210° C., and the extrusion pressure is 7 MPa.

[0099] The preparation method of the modified heavy calcium carbonate is the same as that in Example 1 and will not be repeated here.

[0100] Comparative Example 5:

[0101] A high-toughness and high-filling PP sheet preparation process comprises the following steps:

[0102] (1) 62.5 g of PP, 5.0 g of linear low-density polyethylene, 10.0 g of nano-calcium carbonate, 2.0 g of polyolefin elastomer, 0.5 g of titanate coupling agent TCA-K12, 1 g of PE wax, 0.5 g of antioxidant 168, 10.0 g of glass fiber, 1.0 g of benzotriazole, 3 g of hyperbranched epoxy resin, and 0.5 g of silicone epoxy-modified acrylic resin were added into a high-speed mixer and mixed thoroughly to obtain a uniform mixture at a mixing temperature of 110° C. for 11 min.

[0103] (2) After heating to 115°C, move to a cold mixer and cool the material to 45°C;

[0104] (3) The cooled mixed material of step (2) is heated and extruded through an extruder, and then passes through a sheet die for extrusion molding, and the molded sheet is extruded and shaped through a calender.

[0105] In step (3), the speed of the extruder feeder is the same as the screw speed, both of which are 180 r / min, the die temperature is 170° C., the extruder main engine temperature is 210° C., and the extrusion pressure is 7 MPa.

[0106] Comparative Example 6:

[0107] A high-toughness and high-filling PP sheet preparation process comprises the following steps:

[0108] (1) 42.5 g of PP, 5.0 g of linear low-density polyethylene, 30 g of modified heavy calcium carbonate, 2.0 g of polyolefin elastomer, 0.5 g of titanate coupling agent TCA-K12, 1 g of PE wax, 0.5 g of antioxidant 168, 10.0 g of glass fiber, 1.0 g of benzotriazole, 3 g of hyperbranched epoxy resin, and 0.5 g of silicone epoxy modified acrylic resin were added into a high-speed mixer and mixed thoroughly to obtain a uniform mixture. The mixing temperature was 110° C. and the mixing time was 11 min.

[0109] (2) After heating to 115°C, move to a cold mixer and cool the material to 45°C;

[0110] (3) The cooled mixed material of step (2) is heated and extruded through an extruder, and then passes through a sheet die for extrusion molding, and the molded sheet is extruded and shaped through a calender.

[0111] In step (3), the speed of the extruder feeder is the same as the screw speed, both of which are 180 r / min, the die temperature is 170° C., the extruder main engine temperature is 210° C., and the extrusion pressure is 7 MPa.

[0112] The preparation method of the modified heavy calcium carbonate is the same as that in Example 1 and will not be repeated here.

[0113] Comparative Example 7:

[0114] A high-toughness and high-filling PP sheet preparation process comprises the following steps:

[0115] (1) 34.5 g of PP, 5.0 g of linear low-density polyethylene, 30 g of modified heavy calcium carbonate, 10.0 g of nano calcium carbonate, 0.5 g of titanate coupling agent TCA-K12, 1 g of PE wax, 0.5 g of antioxidant 168, 10.0 g of glass fiber, 1.0 g of benzotriazole, 3 g of hyperbranched epoxy resin, and 0.5 g of silicone epoxy modified acrylic resin were added into a high-speed mixer and mixed thoroughly to obtain a uniform mixture. The mixing temperature was 110° C. and the mixing time was 11 min.

[0116] (2) After heating to 115°C, move to a cold mixer and cool the material to 45°C;

[0117] (3) The cooled mixed material of step (2) is heated and extruded through an extruder, and then passes through a sheet die for extrusion molding, and the molded sheet is extruded and shaped through a calender.

[0118] In step (3), the speed of the extruder feeder is the same as the screw speed, both of which are 180 r / min, the die temperature is 170° C., the extruder main engine temperature is 210° C., and the extrusion pressure is 7 MPa.

[0119] The preparation method of the modified heavy calcium carbonate is the same as that in Example 1 and will not be repeated here.

[0120] Comparative Example 8:

[0121] A high-toughness and high-filling PP sheet preparation process comprises the following steps:

[0122] (1) 42.5 g of PP, 5.0 g of linear low-density polyethylene, 30 g of modified heavy calcium carbonate, 10.0 g of nano calcium carbonate, 2.0 g of polyolefin elastomer, 0.5 g of titanate coupling agent TCA-K12, 1 g of PE wax, 0.5 g of antioxidant 168, 1.0 g of benzotriazole, 3 g of hyperbranched epoxy resin, and 0.5 g of silicone epoxy modified acrylic resin were added into a high mixer and mixed thoroughly to obtain a uniform mixture at a mixing temperature of 110° C. for 11 min;

[0123] (2) After heating to 115°C, move to a cold mixer and cool the material to 45°C;

[0124] (3) The cooled mixed material of step (2) is heated and extruded through an extruder, and then passes through a sheet die for extrusion molding, and the molded sheet is extruded and shaped through a calender.

[0125] In step (3), the speed of the extruder feeder is the same as the screw speed, both of which are 180 r / min, the die temperature is 170° C., the extruder main engine temperature is 210° C., and the extrusion pressure is 7 MPa.

[0126] The preparation method of the modified heavy calcium carbonate is the same as that in Example 1 and will not be repeated here.

[0127] Comparative Example 9:

[0128] A high-toughness and high-filling PP sheet preparation process comprises the following steps:

[0129] (1) 35.5 g of PP, 5.0 g of linear low-density polyethylene, 30 g of modified heavy calcium carbonate, 10.0 g of nano calcium carbonate, 2.0 g of polyolefin elastomer, 0.5 g of titanate coupling agent TCA-K12, 1 g of PE wax, 0.5 g of antioxidant 168, 10.0 g of glass fiber, 1.0 g of benzotriazole, and 0.5 g of silicone epoxy modified acrylic resin were added into a high-speed mixer and mixed thoroughly to obtain a uniform mixture. The mixing temperature was 110° C. and the mixing time was 11 min.

[0130] (2) After heating to 115°C, move to a cold mixer and cool the material to 45°C;

[0131] (3) The cooled mixed material of step (2) is heated and extruded through an extruder, and then passes through a sheet die for extrusion molding, and the molded sheet is extruded and shaped through a calender.

[0132] In step (3), the speed of the extruder feeder is the same as the screw speed, both of which are 180 r / min, the die temperature is 170° C., the extruder main engine temperature is 210° C., and the extrusion pressure is 7 MPa.

[0133] The preparation method of the modified heavy calcium carbonate is the same as that in Example 1 and will not be repeated here.

[0134] Comparative Example 10:

[0135] A high-toughness and high-filling PP sheet preparation process comprises the following steps:

[0136] (1) 33 g of PP, 5.0 g of linear low-density polyethylene, 30 g of modified heavy calcium carbonate, 10.0 g of nano calcium carbonate, 2.0 g of polyolefin elastomer, 0.5 g of titanate coupling agent TCA-K12, 1 g of PE wax, 0.5 g of antioxidant 168, 10.0 g of glass fiber, 1.0 g of benzotriazole, and 3 g of hyperbranched epoxy resin were added to a high-speed mixer and mixed thoroughly to obtain a uniform mixture at a mixing temperature of 110° C. for 11 min;

[0137] (2) After heating to 115°C, move to a cold mixer and cool the material to 45°C;

[0138] (3) The cooled mixed material of step (2) is heated and extruded through an extruder, and then passes through a sheet die for extrusion molding, and the molded sheet is extruded and shaped through a calender.

[0139] In step (3), the speed of the extruder feeder is the same as the screw speed, both of which are 180 r / min, the die temperature is 170° C., the extruder main engine temperature is 210° C., and the extrusion pressure is 7 MPa.

[0140] The preparation method of the modified heavy calcium carbonate is the same as that in Example 1 and will not be repeated here.

[0141] Comparative Example 11:

[0142] A high-toughness and high-filling PP sheet preparation process comprises the following steps:

[0143] (1) 32.5 g of PP, 5.0 g of linear low-density polyethylene, 30 g of modified heavy calcium carbonate, 10.0 g of nano calcium carbonate, 2.0 g of polyolefin elastomer, 0.5 g of titanate coupling agent TCA-K12, 1 g of PE wax, 0.5 g of antioxidant 168, 10.0 g of glass fiber, 1.0 g of benzotriazole, 3 g of hyperbranched polyamide resin, and 0.5 g of silicone epoxy modified acrylic resin were added into a high-speed mixer and mixed thoroughly to obtain a uniform mixture at a mixing temperature of 110° C. for 11 min.

[0144] (2) After heating to 115°C, move to a cold mixer and cool the material to 45°C;

[0145] (3) The cooled mixed material of step (2) is heated and extruded through an extruder, and then passes through a sheet die for extrusion molding, and the molded sheet is extruded and shaped through a calender.

[0146] In step (3), the speed of the extruder feeder is the same as the screw speed, both of which are 180 r / min, the die temperature is 170° C., the extruder main engine temperature is 210° C., and the extrusion pressure is 7 MPa.

[0147] The preparation method of the modified heavy calcium carbonate is the same as that in Example 1 and will not be repeated here.

[0148] Comparative Example 12:

[0149] A high-toughness and high-filling PP sheet preparation process comprises the following steps:

[0150] (1) 39.5 g of PP, 30 g of heavy calcium carbonate, 10.0 g of nano calcium carbonate, 120.5 g of titanate coupling agent TCA-K, 1 g of PE wax, 0.5 g of antioxidant 168, 10.0 g of glass fiber, 1.0 g of benzotriazole, 3 g of hyperbranched polyamide resin, and 0.5 g of acrylic copolymer were added into a high-speed mixer and mixed thoroughly to obtain a uniform mixture at a mixing temperature of 110° C. for 11 min.

[0151] (2) After heating to 115°C, move to a cold mixer and cool the material to 45°C;

[0152] (3) The cooled mixed material of step (2) is heated and extruded through an extruder, and then passes through a sheet die for extrusion molding, and the molded sheet is extruded and shaped through a calender.

[0153] In step (3), the speed of the extruder feeder is the same as the screw speed, both of which are 180 r / min, the die temperature is 170° C., the extruder main engine temperature is 210° C., and the extrusion pressure is 7 MPa.

[0154] Test Example 1: Dimensional change rate test

[0155] The above Example 1 and Comparative Examples 1 to 12 were tested according to ISO 23999 standard.

[0156] Table 1 Test results of dimensional change rate of high-toughness and high-filling PP sheet after heating

[0157]

[0158]

[0159] Modified heavy calcium carbonate is a common method for plastic modification, such as filling modification and reinforcement modification, which can not only greatly reduce costs, but also significantly improve the various properties of plastic products. As can be seen from Table 1, compared with Example 1 and Comparative Examples 5-6, a conclusion can be clearly drawn: the addition of modified heavy calcium carbonate and nano calcium carbonate can well reduce the shrinkage of PP sheets. The possible reasons are: 1. The inorganic filler itself does not shrink, and its addition reduces the shrinkage of the PP sheet as a whole. 2. The addition of inorganic fillers will inevitably affect the crystallinity of PP, thereby affecting the shrinkage. 3. The addition of ultra-fine inorganic fillers plays a certain auxiliary nucleation role, changes the structural state of PP, prevents the formation of large spherulites, and also affects the molding shrinkage of PP. Comparative Example 1 and Comparative Examples 1-3 show that the improvement of the heating dimensional change performance of the silicone epoxy modified acrylic resin for the PP sheet is better than that of acrylic copolymers, epoxy acrylates and polyurethane acrylates. The main factors affecting the heating dimensional change of the PP sheet include the heating expansion of the polypropylene itself, the heating temperature, the cooling conditions, the crystallinity, and the relative humidity. The main factors affecting the crystallinity of PP sheets include raw materials, melt temperature, cooling rate, nucleating agent and processing conditions. Silicone epoxy modified acrylic resin can be used as one of the raw materials of nucleating agent, and a polymer with high-efficiency nucleating effect is generated through polymerization reaction. This polymer can be used as a nucleating agent for PP sheets to improve its crystallization rate and crystallinity, while reducing the amount of nucleating agent added and reducing costs. The side chain of silicone epoxy modified acrylic resin has a polar carboxylate group, and this structure gives it excellent heat oxidation resistance, weather resistance and adhesion. At the same time, in order to improve its cold resistance, water resistance, alkali resistance, etc., organic siloxane is introduced into the main chain of acrylic resin polymer, which can form cross-linked Si-O-Si bonds between polymer macromolecules and between polymer and substrate. This special structure enables it to maintain its stability and performance in harsh environments such as high temperature, low temperature, ultraviolet radiation, and chemical corrosion.

[0160] Test Example 2: Warpage Test

[0161] The above-mentioned Example 1 and Comparative Examples 1 to 12 were subjected to a board warpage test. The normal temperature warpage test conditions were a temperature of 23±2°C and a humidity of 50±5%. The heated warpage test was conducted according to ISO23999, with the temperature adjusted to 70°C and the test performed for 6 hours.

[0162] Table 2 Warpage test results of high-toughness and high-filled PP sheets

[0163]

[0164]

[0165] The main reasons that affect the warping and deformation of the board are roughly as follows: 1. The moisture content of the board: When the moisture content in the board increases, the board will expand; when the ambient humidity is low, the board will shrink; when the drying rate in the board is uneven, the board will warp. 2. The density of the board is unqualified: When the density of the board is too low, the processing surface of the board will be rough and easy to absorb moisture and deform. 3. The production process of the board is not in place: high-quality boards require consistent paving density and symmetrical structure. When the production process of the board is not in place and the difference is too large, the internal expansion and contraction of the board will be inconsistent, resulting in internal stress, which will cause the board to deform. 4. The waterproofness of the board is not good: If the waterproofness of the board itself is not up to standard, it will absorb water and become damp. 5. The maintenance of the board is not up to standard: If the board is not in a relatively dry and ventilated environment, it is easy to affect the stability of the board, resulting in deformation and warping. Possible reasons are: 1. Modified heavy calcium carbonate and silicone epoxy modified acrylic resin can reduce the water absorption of PP boards. 2. The density of the board without modified heavy calcium carbonate is too small. Comparative Example 1 and Comparative Examples 1-3 show that the improvement of the warpage performance of PP sheet by silicone epoxy modified acrylic resin is better than that of acrylic copolymer, epoxy acrylate and polyurethane acrylate. The emulsion particle size distribution of silicone epoxy modified acrylic resin is uniform, the emulsion stability is high, the comprehensive performance of the coating is good, the waterproof performance is good, and the waterproof performance can reach a high level. The waterproof performance of silicone epoxy modified acrylic resin is mainly determined by its chemical structure. Silicone epoxy modified acrylic resin is an emulsion polymer, and its molecular structure contains common units of silicone and acrylate. This molecular structure makes silicone epoxy modified acrylic resin have good waterproof performance. Possible reasons are as follows: First, the silicone unit provides good hydrophobicity in the polymer. This is because the molecular structure of the silicone unit has a lower polarity, which reduces the overall hydrophilicity of the polymer. In contrast, the molecular structure of the acrylate unit has a higher polarity and better hydrophilicity. Therefore, by combining silicone and acrylate, a polymer having both hydrophobicity and good adhesion can be obtained.

[0166] Secondly, the particle size distribution of the silicone epoxy modified acrylic resin emulsion is uniform and the emulsion stability is high. This uniform particle size distribution and stability are conducive to the formation of a dense and uniform waterproof coating.

[0167] In summary, the chemical structure and emulsion properties of silicone epoxy modified acrylic resin jointly determine its good waterproof performance.

[0168] Test Example 3: Impact strength test

[0169] The above Example 1 and Comparative Examples 1 to 12 were subjected to impact strength tests. The impact resistance (room temperature and low temperature impact strength) of the composite material was tested on a Chengde Dahua XJJ-50 impact testing machine according to the national standard GB / T1043.1-2008.

[0170] Table 3 Impact test results of high-toughness and high-filled PP sheets

[0171]

[0172]

[0173] Analysis of Table 3 shows that the PP sheet in Example 1 has the best impact strength, while the PP sheet in Comparative Example 11 has the worst impact strength. Comparison of Example 1 and Comparative Examples 1 to 12 shows that modified heavy calcium carbonate, polyolefin elastomer, hyperbranched epoxy resin, linear low-density polyethylene, acrylate types, etc. can improve the impact strength of PP sheets, but the lack of polyester amide hyperbranched polymer and inorganic modified heavy calcium carbonate will greatly reduce the impact strength of PP sheets. Possible reasons are: modified heavy calcium carbonate increases the hardness and strength of PP sheets; the absence of hyperbranched epoxy resin will affect the synergistic effect and addition amount of each component in the PP sheet and the dispersibility of each component. Silicone epoxy modified acrylic resin is a special polymer that combines the advantages of silicone and acrylate. It has a lower modulus and higher elasticity, and can improve the flexibility and impact strength of PP sheets. It should be noted that the following points should be noted when adding toughening agents: 1. Addition amount. Determine the appropriate addition amount according to the specific requirements of the PP sheet and the characteristics of the toughening agent. 2. Mixing process: Ensure that the toughening agent is fully mixed with the PP resin to ensure that the toughening agent is evenly distributed in the PP sheet. Specifically, the molecular structure of this modified polymer contains two components, silicone and acrylate. The silicone component gives the polymer good heat resistance, weather resistance and low temperature resistance, while the acrylate component gives the polymer excellent weather resistance, UV resistance and chemical corrosion resistance. Through the combination of silicone and acrylate, silicone-modified acrylate can form a cross-linked structure in the PP sheet, improving the impact strength, heat resistance and weather resistance of the PP sheet. In addition, silicone epoxy-modified acrylic resin also has good compatibility and fluidity, and can be well compatible with PP resin and other additives to form a uniform mixture, thereby improving the overall performance of the PP sheet.

[0174] Test Example 4: Tensile and bending strength test

[0175] The tensile and flexural strength tests of the above Example 1 and Comparative Examples 1 to 12 were performed. The tensile strength test of the composite material was performed in accordance with the national standard GB / T 1040.1-2018, with a tensile rate of 10 mm / min; the flexural strength test was performed in accordance with GB / T 9341-2008. The test was performed on a Changchun Kexin WDW 3050 microcomputer-controlled electronic universal testing machine.

[0176] Table 4 Test results of tensile and flexural strength of high-toughness and high-filled PP sheets

[0177] Test items Tensile strength / MPa Bending strength / MPa Example 1 40.0 39.3 Comparative Example 1 27.7 22.3 Comparative Example 2 33.0 31.3 Comparative Example 3 30.8 28.6 Comparative Example 4 33.7 32.9 Comparative Example 5 24.4 23.7 Comparative Example 6 25.5 24.6 Comparative Example 7 35.6 34.1 Comparative Example 8 37.6 36.9 Comparative Example 9 29.9 27.8 Comparative Example 10 31.3 28.7 Comparative Example 11 23.3 21.5 Comparative Example 12 19.9 18.0

[0178] The greater the tensile strength, the better the tensile resistance of the material. When the tensile strength is greater, the material's ability to resist external force damage is stronger, indicating that the material has stronger toughness and strength. Analysis of Example 1 and Comparative Examples 5-6, 11-12 shows that modified heavy calcium carbonate has a direct effect on the tensile and bending strength of PP sheets. Possible reasons: The addition of modified heavy calcium carbonate has a certain reinforcing effect on PP sheets, which increases the bending strength of PP sheets. Analysis of Example 1 and various comparative examples shows that: 1. Modified heavy calcium carbonate and polyester amide hyperbranched polymer have a relatively large effect on the bending tensile strength of PP sheets. 2. The addition of low-density linear polyethylene, nano calcium carbonate, glass fiber nano, polyolefin elastomer and modified calcium carbonate to PP sheets improves its performance, and these substances may play a synergistic role in PP sheets. By analyzing Example 1 and Comparative Examples 1-3, it can be seen that modified acrylates also have a certain tensile and bending strength improvement for PP sheets, and the performance of the silicone epoxy modified acrylic resin of the present invention is better than that of several other modified acrylates.

[0179] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Modifications, replacements, and improvements made within the principles of the present invention should all be included in the protection scope of the present invention.

Claims

1. A high-toughness and high-filling PP sheet, characterized in that: The composition comprises the following components by weight: 30-40 parts of PP, 1-10 parts of linear low-density polyethylene, 20-40 parts of modified heavy calcium carbonate, 8-15 parts of nano calcium carbonate, 1-3 parts of polyolefin elastomer, 0.1-1 parts of coupling agent, 0.1-2 parts of lubricant, 0.1-1 parts of antioxidant, 10-20 parts of glass fiber, 0.1-3 parts of light stabilizer, 2-5 parts of hyperbranched epoxy resin, and 0.1-1 parts of silicone epoxy modified acrylic resin; The modified heavy calcium carbonate preparation steps are as follows: (1) Weigh 20-30 g of heavy calcium carbonate, add 50-100 mL of water and anhydrous ethanol, the volume ratio of water to anhydrous ethanol is 1:3, then stir at a speed of 800-1000 r / min to form a suspension, and then heat the suspension; (2) When the temperature reaches 60-70° C., add 10-20 g of sodium stearate into the reaction bottle containing the heavy calcium carbonate suspension and stir to react for 40-50 min; (3) After the reaction is completed, the product is repeatedly washed with water and anhydrous ethanol for multiple times, filtered and separated, and vacuum dried at 50-60° C. for 24-30 hours to obtain modified heavy calcium carbonate; Silicone epoxy modified acrylic resin, model: SJ-804, source: Jining Tangyi Chemical Co., Ltd.

2. The high-toughness and high-filling PP sheet according to claim 1, characterized in that: The average particle size of the nano calcium carbonate is 10 to 30 nm.

3. The high-toughness and high-filling PP sheet according to claim 1, characterized in that: The polyolefin elastomer is at least one of ethylene-octene copolymer and ethylene-propylene copolymer.

4. The high-toughness and high-filling PP sheet according to claim 1, characterized in that: The coupling agent is at least one of titanate coupling agent, aluminate coupling agent and silane coupling agent; the lubricant is at least one of stearic acid, paraffin, PE wax, stearate, monoglyceride, PETS, EBS and TAF lubricants; the antioxidant is at least one of antioxidant 1010 and antioxidant 168; the glass fiber is alkali-free, with a single fiber diameter of 11 to 17 μm and a particle size of 10 to 350 μm; the light stabilizer is at least one of zinc phosphate, benzotriazole, acrylic acid and triazine.

5. A process for preparing a high-toughness and high-filling PP sheet according to any one of claims 1 to 4, characterized in that: The steps are as follows: (1) adding 30-40 parts by weight of PP, 1-10 parts by weight of linear low-density polyethylene, 20-40 parts by weight of modified heavy calcium carbonate, 8-15 parts by weight of nano calcium carbonate, 1-3 parts by weight of polyolefin elastomer, 0.1-1 parts by weight of coupling agent, 0.1-2 parts by weight of lubricant, 0.1-1 parts by weight of antioxidant, 10-20 parts by weight of glass fiber, 0.1-3 parts by weight of light stabilizer, 2-5 parts by weight of hyperbranched epoxy resin, and 0.1-1 parts by weight of silicone epoxy modified acrylic resin into a high-speed mixer and mixing thoroughly to obtain a uniform mixture at a mixing temperature of 90-120° C. for a mixing time of 8-15 min; (2) After heating to 110-120°C, move to a cold mixer and cool the material to 40-60°C; (3) The cooled mixed material of step (2) is heated and extruded through an extruder, and then passes through a sheet die for extrusion molding, and the molded sheet is extruded and shaped through a calender.

6. A process for preparing a high-toughness and high-filling PP sheet according to claim 5, characterized in that: In step (3), the speed of the extruder feeder and the screw speed are 150-250 r / min, the die temperature is 150-200° C., the temperature of the extruder main engine is 190-230° C., and the extrusion pressure is 5-8 MPa.

7. Use of a high-toughness and high-filling PP board according to any one of claims 1 to 4 in making floors.