A kind of sacrificial red glaze ceramic and preparation method
By mixing under a reducing atmosphere during the frit preparation stage and firing under a nitrogen atmosphere, the problem of changing glaze color of the red glaze ceramics is solved, the yield rate and preparation stability are improved, and the glaze hardness and gloss are achieved Improvement of degree.
Patent Information
- Application Number
- CN202311352503.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-18
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-10-18
AI Technical Summary
In the prior art, the glaze color is variable and difficult to control during the preparation process of the sacred glaze ceramic, resulting in low yield and strict control of firing conditions, making it difficult to achieve large-scale mass production.
During the frit preparation stage, the raw glaze powder is mixed in a reducing atmosphere and made into a frit with the same color. The frit is then broken, water is added to make a glaze slurry, and fired under a nitrogen or an inert gas atmosphere. Avoid secondary oxidation and ensure stable glaze color.
The preparation of red glaze ceramics with consistent glaze color and soft moistness has been achieved, which significantly improves the yield rate and simplifies the preparation process, making the glaze surface hardness, good gloss and more exquisite appearance.
Smart Images

Figure CN117383966B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of daily-use and artistic ceramics, and in particular to a sacrificial red glaze ceramic and a preparation method thereof. Background Art
[0002] With the development of the times, people's pursuit of aesthetics and art has been continuously improved. Colored glazes show the art of earth and fire to the fullest, so they are more and more popular. As a ceramic decorative material, high-temperature colored glaze has good corrosion resistance and strong alkali resistance. In recent years, it has been widely used in ordinary daily-use porcelain and ceramic cultural tourism products, among which personalized tableware is the most common. There are many types of high-temperature colored glazes, which are mainly divided into three color glaze systems: one is the green glaze system with iron as the main colorant; the second is the blue glaze system with cobalt as the main colorant; the third is the copper red glaze system with copper as the main colorant. The colored glazes of these three systems are fired in a high-temperature reducing atmosphere. Among them, the high-temperature color of the representative shadow blue of the green glaze system and the representative Jilan of the blue glaze system are relatively stable. They are the two high-temperature colored glazes with a high market share of high-temperature colored glazes. As a "treasure" among high-temperature colored glazes, copper red glaze is famous for its colorful glaze colors. It has been very rare since ancient times and is deeply loved by people, but its firing is the most difficult "art of fire" to master. Typical representatives of copper red glazes are Jihong, Junhong and Langyaohong. Among these three copper red glazes, Jihong is the most difficult to fire and has the lowest yield rate, which greatly limits its large-scale mass production.
[0003] For a long time, many experts and scholars at home and abroad have conducted tireless research on sacrificial red glaze. The research results on its coloring mechanism include Cu 2 O colloid coloring, elemental copper agglomeration to make the glaze red, and liquid-liquid phase separation to make the copper element distributed in a certain microphase to color. From the color development mechanism of the sacrificial red glaze, it can be seen that at high temperature, under the action of reducing atmosphere, CuO in the glaze is reduced to Cu 2 O and Cu exist in the glaze in the form of colloidal particles. During the firing process of the sacrificial red glaze, on the one hand, it is necessary to control the Cu 2 On the one hand, the content and distribution of O and Cu colloidal particles must be ensured, and on the other hand, the glaze must not be secondary oxidized after firing, which is particularly important for the stable color of the sacrificial red glaze. Therefore, there are many conditions to control during the firing process of the sacrificial red glaze, such as heating rate, oxidizing atmosphere, reducing atmosphere, etc. If the above conditions are not accurately controlled, the color of the sacrificial red glaze will be unstable and impure.
[0004] At present, domestic scholars have imitated the coloring mechanism of sacrificial red glaze in various ways based on the research results. Although the yield of sacrificial red glaze ceramics has been improved to a certain extent, the firing conditions need to be strictly controlled during the preparation process to achieve consistent color, which is difficult for mass production, and it takes a lot of time, manpower and energy to ensure consistent color. Therefore, the above methods all solve the technical problems of variable glaze color and difficult to control glaze color during the preparation of sacrificial red glaze ceramics by controlling the conditions during the firing process, and none of them solves the problem fundamentally. Summary of the invention
[0005] The present invention aims at the problem that the glaze color is changeable and difficult to control in the preparation process of sacrificial red glaze ceramics in the prior art, and proposes a sacrificial red glaze ceramic and a preparation method. In the frit preparation stage, a raw material glaze powder mixture is made into a frit with uniform color under a reducing atmosphere to control the color of the sacrificial red glaze ceramic. The sacrificial red glaze ceramic prepared by the method has not only uniform color, moist and soft luster, but also a clean glaze surface without cracks, and also improves the yield of the sacrificial red glaze ceramic.
[0006] In order to achieve the above technical purpose, the present invention provides a method for preparing sacrificial red glaze ceramics, comprising the following steps:
[0007] S1. Preparation of raw glaze powder: mixing the base glaze with the colorant and the reducing auxiliary agent to obtain the raw glaze powder;
[0008] S2, preparation of frit: melting and cooling the raw material glaze powder mixture under a reducing atmosphere to obtain a frit;
[0009] S3, preparation of frit glaze slurry: crushing the frit, adding water and grinding to obtain frit glaze slurry;
[0010] S4, glazing: applying glaze slurry on the body, and then drying the body to obtain a green body;
[0011] S5, firing: placing the green body in an atmosphere of nitrogen and / or inert gas for firing, cooling, and obtaining a sacrificial red glaze ceramic product.
[0012] The components of the base glaze include kaolin, feldspar, quartz and calcite.
[0013] Preferably, based on the mass percentage of the basic glaze being 100%, the basic glaze comprises 8%-12% kaolin, 54%-58% feldspar, 22%-26% quartz and 12%-15% calcite.
[0014] More preferably, based on the mass percentage of the basic glaze being 100%, the basic glaze comprises 8% kaolin, 55% feldspar, 22% quartz and 15% calcite.
[0015] More preferably, based on the mass percentage of the basic glaze being 100%, the basic glaze comprises 9% kaolin, 55% feldspar, 23% quartz and 13% calcite.
[0016] More preferably, based on the mass percentage of the basic glaze being 100%, the basic glaze comprises 12% kaolin, 54% feldspar, 22% quartz and 12% calcite.
[0017] The colorant is selected from one or more of copper oxide, copper carbonate, and copper hydroxide, and the amount of the colorant is 0.3%-0.8% of the mass of the base glaze; and / or the reducing auxiliary agent includes tin oxide, and the amount of the reducing auxiliary agent is 0.5%-1.5% of the mass of the base glaze.
[0018] In step S2, the reducing atmosphere is selected from one or both of carbon monoxide and hydrogen; and / or the melting temperature is 1500°C-1600°C.
[0019] In step S3, the amount of water used is 38%-42% of the mass of the frit.
[0020] The grinding method is ball milling, the ball milling speed is 350rpm-480rpm, and the time is 2h-4h.
[0021] Preferably, the frit is sieved after ball milling, and the aperture of the sieve is 160-325 mesh.
[0022] In step S4, the glazing method is selected from one of dipping glaze and spraying glaze; and / or the glazing thickness is 0.3mm-0.5mm; and / or the drying temperature is 100℃-110℃, and the drying time is 4h-6h.
[0023] In step S5, the sintering temperature is 1250°C-1300°C, and the sintering time is 8h-10h.
[0024] The inert gas is selected from one or both of argon and helium; preferably, the sintering atmosphere is nitrogen and / or argon.
[0025] The invention also provides a sacrificial red glaze ceramic.
[0026] The technical solution of the present invention has the following beneficial effects:
[0027] (1) The present invention provides a method for preparing sacrificial red glaze ceramics, comprising the following steps: S1, preparation of raw glaze powder: taking a base glaze and mixing it with a colorant and a reducing auxiliary agent to obtain raw glaze powder; S2, preparation of frit: melting and cooling the raw glaze powder mixture under a reducing atmosphere to obtain a frit; S3, preparation of frit glaze slurry: crushing the frit, grinding it with water to obtain a frit glaze slurry; S4, glazing: applying the glaze slurry to the body, and then drying the body to obtain a green body; S5, firing: placing the green body in an atmosphere of nitrogen and / or inert gas for firing, cooling, and obtaining a sacrificial red glaze ceramic product. In the method of the present invention, the raw glaze powder mixture is first prepared into a frit with consistent color under a reducing atmosphere; the frit is used to make a glaze slurry and applied to the body, and a nitrogen and / or inert gas atmosphere is used during firing, thereby avoiding the situation of inconsistent color caused by secondary oxidation, making the color stable, and greatly improving the yield rate. Therefore, the method of the present invention can be used to prepare sacrificial red glaze ceramics with consistent and stable glaze color, which greatly simplifies the preparation process and improves the yield rate.
[0028] (2) The present invention provides a method for preparing sacrificial red glaze ceramics. By selecting 8%-12% kaolin, 54%-58% feldspar, 22%-26% quartz and 12%-15% calcite as the base glaze, the prepared sacrificial red glaze ceramics have high glaze hardness, good glossiness and more exquisite appearance. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0030] Figure 1 It is a schematic diagram of the appearance of the sacrificial red glaze ceramic prepared in Example 1 of the present invention.
[0031] Figure 2 It is a schematic diagram of the appearance of the sacrificial red glaze ceramic prepared in the comparative example 1 of the present invention in an oxygen atmosphere.
[0032] Figure 3 This is a schematic diagram of the appearance of the sacrificial red glaze ceramic prepared in comparative example 2 of the present invention in a carbon monoxide atmosphere.
[0033] Figure 4 This is a schematic diagram of the appearance of the sacrificial red glaze ceramic prepared in the comparative example 3 of the present invention in an oxidizing atmosphere for preparing the frit.
[0034] Figure 5This is a schematic diagram of the appearance of the sacrificial red glaze ceramic prepared by wet ball grinding of raw material glaze powder in comparative example 4 of the present invention and firing in an atmosphere of 5% (volume percentage) carbon monoxide and 95% (volume percentage) air. DETAILED DESCRIPTION
[0035] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0036] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0037] Example 1
[0038] This embodiment provides a method for preparing sacrificial red glaze ceramics, comprising the following steps:
[0039] S1. Preparation of raw glaze powder: 8 kg of kaolin, 55 kg of feldspar, 22 kg of quartz, 15 kg of calcite, 0.3 kg of copper oxide, and 0.5 kg of tin oxide are weighed and mixed to obtain raw glaze powder;
[0040] S2, preparation of frit: putting raw material glaze powder into a mixer for stirring and mixing, placing the mixed raw material glaze powder into a kiln, melting it at 1500° C. in a carbon monoxide atmosphere, and cooling it to obtain a frit after the raw material glaze powder is evenly melted;
[0041] S3, preparation of frit glaze slurry: after the above frit is crushed, it is placed in a ball mill, and 38% of the mass of the frit is added with water for ball milling, the ball milling speed is 420rpm, the time is 3h, and the ball milling fineness reaches: the residue on the 325-mesh standard sieve is less than 0.02%, and the frit glaze slurry is obtained after passing through the 180-mesh standard sieve;
[0042] S4, glazing: applying the frit glaze slurry on the body by dipping glaze method, the glazing thickness is 0.5mm, and the glazed body is placed in an oven at 100°C and dried for 5 hours to obtain a green body;
[0043] S5. Firing: Place the green body in a nitrogen atmosphere kiln and fire at 1250°C for 9 hours. After cooling, the sacrificial red glaze ceramic product is obtained.
[0044] Example 2
[0045] This embodiment provides a preparation method of sacrificial red glaze ceramics, which differs from Example 1 in that: the raw glaze powder formula in step S1 is 8Kg of kaolin, 58Kg of feldspar, 22Kg of quartz, 12Kg of calcite, 0.5Kg of copper oxide, and 0.8Kg of tin oxide; the amount of water used in step S3 is 40% of the mass of the frit; the glazing thickness in step S4 is 0.4mm, and the rest of the preparation method is consistent with Example 1.
[0046] Example 3
[0047] The present embodiment provides a method for preparing sacrificial red glaze ceramics, which differs from Example 1 in that: the raw glaze powder formula in step S1 is 9Kg of kaolin, 55Kg of feldspar, 23Kg of quartz, 13Kg of calcite, 0.5Kg of copper oxide, and 1.0Kg of tin oxide; the melting temperature of the frit in step S2 is 1580°C; the amount of water used in step S3 is 42% of the mass of the frit; the glazing thickness in step S4 is 0.3mm; the firing atmosphere in step S5 is argon atmosphere, and the firing temperature is 1280°C. The rest of the preparation method is consistent with Example 1.
[0048] Example 4
[0049] The present embodiment provides a method for preparing sacrificial red glaze ceramics, which differs from Example 1 in that: the raw glaze powder formula in step S1 is 8Kg of kaolin, 54Kg of feldspar, 26Kg of quartz, 12Kg of calcite, 0.5Kg of copper oxide, and 1.0Kg of tin oxide; the melting temperature of the frit in step S2 is 1580°C; the amount of water used in step S3 is 42% of the mass of the frit; the glazing thickness in step S4 is 0.4mm; the firing atmosphere in step S5 is argon atmosphere, and the firing temperature is 1280°C. The rest of the preparation method is consistent with Example 1.
[0050] Example 5
[0051] The present embodiment provides a method for preparing sacrificial red glaze ceramics, which differs from Example 1 in that: the raw glaze powder formula in step S1 is 12Kg of kaolin, 54Kg of feldspar, 22Kg of quartz, 12Kg of calcite, 0.8Kg of copper oxide, and 1.5Kg of tin oxide; the melting temperature of the frit in step S2 is 1600°C; the amount of water used in step S3 is 42% of the mass of the frit; the glazing thickness in step S4 is 0.3mm; the firing temperature in step S5 is 1300°C, and the rest of the preparation method is consistent with Example 1.
[0052] Example 6
[0053] The present embodiment provides a method for preparing sacrificial red glaze ceramics, which differs from Example 1 in that: the raw glaze powder formula in step S1 is 12Kg of kaolin, 54Kg of feldspar, 22Kg of quartz, 12Kg of calcite, 0.8Kg of copper oxide, and 1.5Kg of tin oxide; the melting temperature of the frit in step S2 is 1600°C; the amount of water used in step S3 is 42% of the mass of the frit; the glazing thickness in step S4 is 0.3mm; the firing atmosphere in step S5 is nitrogen and argon (volume ratio 1:1), and the firing temperature is 1300°C. The rest of the preparation method is consistent with Example 1.
[0054] Comparative Example 1
[0055] This comparative example provides a method for preparing ceramics, which differs from Example 1 in that the firing atmosphere in step S5 is oxygen, and the amounts of other raw materials and process parameters are consistent with those in Example 1.
[0056] Comparative Example 2
[0057] This comparative example provides a method for preparing ceramics, which is different from Example 1 in that the firing atmosphere in step S5 is carbon monoxide, and the amounts of other raw materials and process parameters are consistent with those in Example 1.
[0058] Comparative Example 3
[0059] This comparative example provides a method for preparing ceramics, which is different from Example 1 in that the atmosphere for preparing the frit in step S2 is oxygen, and the amounts of other raw materials and process parameters are consistent with those in Example 1.
[0060] Comparative Example 4
[0061] This comparative example provides a method for preparing sacrificial red glaze ceramics, which differs from Example 1 in that: step S2 is not performed; in step S3, the raw glaze powder is wet-milled with water until the fineness is 0.01% on a 325-mesh standard sieve, to obtain a glaze slurry; in step S5, the firing atmosphere is 5% (volume percentage) carbon monoxide and 95% (volume percentage) air; the remaining raw material amounts and process parameters are consistent with those in Example 1.
[0062] Ceramics were prepared according to the methods of Examples 1-6 and Comparative Examples 1-4, respectively. 50 batches of ceramics were prepared in each group and evaluated externally. If the glaze of the sacrificial red glaze ceramic was bright, crack-free, pure red, uniform and delicate, it was recorded as a finished product. Otherwise, it was recorded as a defective product. The yield of the 50 sacrificial red glaze ceramics prepared in each group was calculated.
[0063] Table 1 Summary of sacrificial red glaze ceramics
[0064]
[0065] The sacrificial red glaze ceramics prepared in Examples 1-6 of the present invention mostly meet the requirements of bright glaze, no cracks, pure red color, uniform and delicate, and the yield rate reaches 91-95%. Figure 1 The colors of the comparative examples 1-3 are green or grayish black, without the red effect. Figure 2-4 . This indicates that the use of different gas atmospheres in the firing step leads to Figure 1-4 The color of the red glaze ceramics is quite different. In addition, compared with the traditional raw glaze reduction atmosphere firing ( Figure 5 ), the sacrificial red glaze ceramics prepared by the present invention have a purer glaze color and a higher yield rate. Therefore, the preparation method of the present invention can be used to prepare sacrificial red glaze ceramics with a pure glaze color and a high yield rate.
Claims
1. A method for preparing sacrificial red glaze ceramics, characterized in that: The following steps are involved: S1. Preparation of raw glaze powder: Mix the base glaze with the colorant and the reducing auxiliary agent to obtain the raw glaze. Powder; based on the mass percentage of the basic glaze being 100%, the basic glaze comprises 8%-12% kaolin, 54%-58% feldspar, 22%-26% quartz and 12%-15% calcite; S2. Preparation of frit: melting and cooling the raw material glaze powder mixture under a reducing atmosphere to obtain a frit; the reducing atmosphere is selected from one or both of carbon monoxide and hydrogen; S3, preparation of frit glaze slurry: crushing the frit, adding water and grinding to obtain frit glaze slurry; S4, glazing: applying glaze slurry on the body, and then drying the body to obtain a green body; S5, firing: placing the green body in an atmosphere of nitrogen and / or inert gas for firing, cooling, and obtaining a sacrificial red glaze ceramic product.
2. The method for preparing sacrificial red glaze ceramics according to claim 1, characterized in that: Taking the mass percentage of the basic glaze as 100%, the basic glaze includes 8% kaolin, 55% feldspar, 22% quartz and 15% calcite; or, includes 9% kaolin, 55% feldspar, 23% quartz and 13% calcite; or, includes 12% kaolin, 54% feldspar, 22% quartz and 12% calcite.
3. The method for preparing sacrificial red glaze ceramics according to claim 1 or 2, characterized in that: The colorant is selected from one or more of copper oxide, copper carbonate, and copper hydroxide, and the amount of the colorant is 0.3%-0.8% of the mass of the basic glaze.
4. The method for preparing sacrificial red glaze ceramics according to claim 1 or 2, characterized in that: The reducing auxiliary agent includes tin oxide, and the amount of the reducing auxiliary agent is 0.5%-1.5% of the mass of the basic glaze.
5. The method for preparing sacrificial red glaze ceramics according to claim 1 or 2, characterized in that: In step S2, the melting temperature is 1500°C-1600°C.
6. The method for preparing sacrificial red glaze ceramics according to claim 1 or 2, characterized in that: In step S3, the amount of water used is 38%-42% of the mass of the frit.
7. The method for preparing sacrificial red glaze ceramics according to claim 1 or 2, characterized in that: In step S3, the grinding method is ball milling, the ball milling speed is 350rpm-480rpm, and the time is 2h-4h.
8. The method for preparing sacrificial red glaze ceramics according to claim 7, characterized in that: The frit is sieved after ball milling, and the aperture of the sieve is 160 meshes to 325 meshes.
9. The method for preparing sacrificial red glaze ceramics according to claim 1 or 2, characterized in that: In step S4, the glazing method is selected from one of dipping glaze and spraying glaze.
10. The method for preparing sacrificial red glaze ceramics according to claim 1 or 2, characterized in that: In step S4, the glazing thickness is 0.3 mm-0.5 mm.
11. The method for preparing sacrificial red glaze ceramics according to claim 1 or 2, characterized in that: In step S4, the drying temperature is 100° C.-110° C., and the drying time is 4 h-6 h.
12. The method for preparing sacrificial red glaze ceramics according to any one of claims 1 or 2, characterized in that: In step S5, the sintering temperature is 1250°C-1300°C, and the sintering time is 8h-10h.
13. The method for preparing sacrificial red glaze ceramics according to claim 1 or 2, characterized in that: In step S5, the inert gas is selected from one or both of argon and helium.
14. The method for preparing sacrificial red glaze ceramics according to claim 1 or 2, characterized in that: In step S5, the sintering atmosphere is nitrogen and / or argon.
15. A sacrificial red glaze ceramic prepared according to the method according to any one of claims 1 to 14.