A wide temperature range dimming film with low off-axis haze and its preparation method and application
By using a three-layer liquid crystal/polymer composite material in the PDLC film, combining ultraviolet light polymerizable monomers and gap particles, the problem of high haze in the PDLC film at a large observation angle in the prior art is solved, and the low Off-axis haze and wide temperature-diffusing films with wide viewing angles enhance their application value in car windows and building windows.
Patent Information
- Application Number
- CN202311435631.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-11-01
AI Technical Summary
When the existing PDLC films have a large observation angle, the effective refractive index of liquid crystal droplets is mismatched with the refractive index of polymer, resulting in an increase in haze, limiting their application in car windows and building windows.
A low off-axis haze wide temperature domain dimming film with a three-layer structure includes three layers, including upper, middle and lower layers, where the upper and lower layers are conductive glass or conductive plastic films, and the intermediate layer is liquid crystal/polymer composite material. The birefringence of the mixed liquid crystal is between 0.1 and 0.15, combined with ultraviolet light, polymerizes monomers and gap particles, and cures by ultraviolet light to form a wide temperature dimming film with low off-axis haze.
Maintaining high open light transmittance and low haze at a wide observation angle reduces the mismatch between the refractive index of liquid crystal droplets and polymers, is suitable for high-temperature and low-temperature environments, and improves the application value of dimming films , especially suitable for automotive smart windows and building doors and windows.
Smart Images

Figure CN117434757B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of functional liquid crystal materials, and specifically relates to a wide-temperature range dimming film with low off-axis haze, and a preparation method and application thereof. Background Art
[0002] Polymer dispersed liquid crystal (PDLC) film is an electrically controlled liquid crystal dimming film that combines the excellent mechanical and thermal properties of polymers with the external field stimulation response characteristics of liquid crystals. It has the advantages of high sensitivity and fast response time. It can be prepared into large-area films of various shapes and thicknesses and is widely used in automobile windows and building windows.
[0003] In the PDLC film, the liquid crystal is evenly dispersed in the polymer matrix in the form of droplets. In the absence of an electric field, the directors of the liquid crystal molecules are randomly distributed. Due to the mismatch between the refractive index of the liquid crystal molecules and the polymer matrix, the PDLC film is in a light scattering state. After the electric field is applied, the directors of the liquid crystal molecules are uniformly oriented along the direction of the electric field. At this time, the refractive index of the liquid crystal droplets matches the refractive index of the polymer matrix, and the PDLC film is transparent. The PDLC film can adjust the transmittance of the window at any time through the change of the liquid crystal layer, and automatically adjust the brightness of the window according to the intensity of the external light. It can not only meet the sun protection needs, but also maintain a good field of vision, improve the comfort of the driver and passengers in the car, and also help improve driving safety.
[0004] However, due to the optical anisotropy of liquid crystal materials in existing PDLC films, as the observation angle increases, the effective refractive index of the liquid crystal droplets in the dimming film becomes mismatched with the refractive index of the polymer, resulting in a decrease in the on-state transmittance of the film and an increase in haze when the observation angle is large, which restricts the application of PDLC films in car windows and building windows. Summary of the invention
[0005] The present application provides a wide temperature range dimming film with low off-axis haze and a preparation method and application thereof. The prepared dimming film has a wide viewing angle and low haze, aiming to solve the problem of narrow viewing angle and high haze of the dimming film in the prior art.
[0006] In order to achieve the above objectives, the present application adopts the following technical solutions.
[0007] On one hand, the present application provides a wide temperature range dimming film with low off-axis haze, comprising an upper layer, a middle layer and a lower layer stacked in a layered manner along the thickness direction, wherein the upper layer and the lower layer are conductive glass or conductive plastic film, and the middle layer is a liquid crystal / polymer composite material, wherein the liquid crystal / polymer composite material comprises a mixed liquid crystal, an ultraviolet light polymerizable monomer, a photoinitiator and interstitial particles;
[0008] The mixed liquid crystal has a birefringence greater than 0.1 and less than 0.15, a crystallization point less than -40°C, a clearing point greater than 120°C, a viscosity less than 80 mPas, and a dielectric anisotropy greater than 3.
[0009] In some embodiments, the hybrid liquid crystal includes a wide temperature range liquid crystal and a low birefringence liquid crystal;
[0010] The wide temperature range liquid crystal is a nematic phase liquid crystal, with a birefringence greater than 0.18, a crystallization point less than -40°C, a clearing point greater than 120°C, and a viscosity less than 80 mPas;
[0011] The low birefringence liquid crystal is a positive nematic phase liquid crystal, and its birefringence is ≤0.1;
[0012] In the mixed liquid crystal, the wide temperature range liquid crystal accounts for 62 to 24 parts, and the low birefringence liquid crystal accounts for 38 to 76 parts.
[0013] In some embodiments, the low birefringence liquid crystal comprises the following compounds:
[0014]
[0015] Wherein, R1 and R2 are groups -F or -CN, and R3 is selected from an alkyl group having 3 to 7 carbon atoms.
[0016] In some embodiments, the liquid crystal / polymer composite material comprises, by weight, 50.0 to 80.0 parts of mixed liquid crystal and 50.0 to 20.0 parts of ultraviolet light polymerizable monomer;
[0017] The initiator and the gap particles account for 1-0.5 wt% and 0.2-0.5 wt% of the total mass of the mixed liquid crystal and the ultraviolet light polymerizable monomer respectively.
[0018] In some embodiments, the UV-polymerizable monomer is a mixture of one or more of epoxy acrylate, polyurethane acrylate, polyester acrylate, epoxy acrylate, polyene thiol system, polyether acrylate, and vinyl ether.
[0019] In some embodiments, the photoinitiator is at least one of benzoin ethyl ether, 2-hydroxy-2-methyl-1-phenylpropanone, trimethylbenzoyldiphenylphosphine oxide, and benzoin diethyl ether.
[0020] In some embodiments, the thickness of the liquid crystal / polymer composite material is 10-20 μm, and the diameter of the interstitial particles is 10-20 μm.
[0021] Another aspect of the present application provides a method for preparing a wide temperature range dimming film with low off-axis haze, comprising:
[0022] S1, mixing a mixed liquid crystal, an ultraviolet light polymerizable monomer, interstitial particles and a photoinitiator, and stirring them evenly to form a prepolymer solution;
[0023] S2, pouring the prepolymer liquid into the middle of two parallel conductive glass or conductive plastic films, curing by ultraviolet light irradiation, and obtaining a wide temperature range dimming film with low off-axis haze.
[0024] In some embodiments, the UV curing time is 100 to 300 seconds, and the UV intensity is 15 to 30 mW / cm 2 .
[0025] The third aspect of the present application provides the use of the wide temperature range dimming film with low off-axis haze or the wide temperature range dimming film with low off-axis haze prepared by the above preparation method on automobile windows or building windows.
[0026] Compared with the prior art, the beneficial effects of this application are:
[0027] The wide temperature range dimming film with low off-axis haze of the present application has low birefringence, low rotational viscosity, low crystallization point and high-definition bright spots, and has high open-state light transmittance and low haze at a wider viewing angle. At a 0-degree viewing angle, the haze is only 2.4%, and at a viewing angle of plus or minus 60 degrees, the haze is 11.9%. The wide temperature range dimming film with low off-axis haze of the present application effectively reduces the mismatch between the effective refractive index of the liquid crystal droplets and the refractive index of the polymer at a large viewing angle, thereby reducing the off-axis haze, and has good application and viewing angle comfort in both high and low temperature environments, greatly improving the outdoor application value of the dimming film, especially suitable for automotive smart windows and building doors and windows and other fields.
[0028] The method for preparing the wide-temperature-range dimming film with low off-axis haze of the present application is simple and easy to operate, has a mild and controllable reaction, and a short curing time, which is conducive to large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments recorded in the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0030] Figure 1 1 is an observation angle-transmittance curve and a haze data diagram of the dimming film prepared in Comparative Example 1;
[0031] Figure 2 2 is the voltage-transmittance curve of the dimming film prepared in Comparative Example 1 at different temperatures;
[0032] Figure 3 2. The observation angle-transmittance curve and haze data diagram of the dimming film prepared in Comparative Example 2;
[0033] Figure 4 2 is the voltage-transmittance curve of the dimming film prepared in Comparative Example 2 at different temperatures;
[0034] Figure 5 1 is an observation angle-transmittance curve and a haze data diagram of the dimming film prepared in Example 1;
[0035] Figure 6 1 is the voltage-transmittance curve of the dimming film prepared in Example 1 at different temperatures;
[0036] Figure 7 2 is an observation angle-transmittance curve and a haze data diagram of the dimming film prepared in Example 2;
[0037] Figure 8 2 is the voltage-transmittance curve of the dimming film prepared in Example 2 at different temperatures;
[0038] Fig. 9 1 is an observation angle-transmittance curve and a haze data diagram of the dimming film prepared in Example 3;
[0039] Fig.10 3 is the voltage-transmittance curve of the dimming film prepared in Example 3 at different temperatures;
[0040] Fig.11 The actual pictures are of the dimming films prepared in Examples 1-3 and Comparative Examples 1-2 at observation angles of 0° and ±60°. DETAILED DESCRIPTION
[0041] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0042] In the following description of this embodiment, the terms "include", "comprising", "having" and "containing" are all open terms, meaning including but not limited to.
[0043] In the following description of this embodiment, the term "and / or" is used to describe the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, B exists alone, and A and B exist at the same time. A and B can be singular or plural. The character " / " generally indicates that the associated objects before and after are in an "or" relationship.
[0044] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0045] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0046] Those skilled in the art should understand that in the following description of the embodiments of the present application, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0047] Those skilled in the art will appreciate that the numerical ranges in the embodiments of the present application are to be understood as each intermediate value between the upper and lower limits of the scope also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present application. The upper and lower limits of these smaller ranges may be independently included or excluded in the scope.
[0048] Unless otherwise specified, the technical / scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which this application belongs. Although this application only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of this application. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0049] The present application provides a wide temperature range dimming film with low off-axis haze, comprising an upper layer, a middle layer and a lower layer stacked in a layered manner along the thickness direction, wherein the upper layer and the lower layer are conductive glass or conductive plastic film, and the middle layer is a liquid crystal / polymer composite material, characterized in that the liquid crystal / polymer composite material comprises a mixed liquid crystal, an ultraviolet light polymerizable monomer, a photoinitiator and interstitial particles;
[0050] The mixed liquid crystal has a birefringence greater than 0.1 and less than 0.15, a crystallization point less than -40°C, a clearing point greater than 120°C, a viscosity less than 80 mPas, and a dielectric anisotropy greater than 3.
[0051] The wide temperature range dimming film with low off-axis haze of the present application has low birefringence, low rotational viscosity, low crystallization point and high-definition bright spots, and has high open-state light transmittance and low haze at a viewing angle of plus or minus 60 degrees. At a viewing angle of 0 degrees, the haze is only 2.4%, and at a viewing angle of plus or minus 60 degrees, the haze is 11.9%. The wide temperature range dimming film with low off-axis haze of the present application effectively reduces the mismatch between the effective refractive index of the liquid crystal droplets and the refractive index of the polymer at a large viewing angle, thereby reducing the off-axis haze of the dimming film, and has good application and viewing angle comfort in both high and low temperature environments, greatly improving the outdoor application value of the electrically controlled liquid crystal dimming film, and is particularly suitable for automotive smart windows and building doors and windows and other fields.
[0052] In the present application, the mixed liquid crystal includes a wide temperature range liquid crystal and a low birefringence liquid crystal; the wide temperature range liquid crystal is a nematic phase liquid crystal, and its birefringence is greater than 0.18, the crystallization point is less than -40°C, the clearing point is greater than 120°C, and the viscosity is less than 80mPas; the low birefringence liquid crystal is a positive nematic phase liquid crystal, and its birefringence is ≤0.1. The mixed liquid crystal is prepared by compounding the wide temperature range liquid crystal and the low birefringence liquid crystal, and the refractive index difference between the mixed liquid crystal and the polymer matrix is reduced, which effectively reduces the off-axis haze of the dimming film.
[0053] Specifically, the low birefringence liquid crystal includes the following compounds:
[0054]
[0055]
[0056] Wherein, R1 and R2 are groups -F or -CN, and R3 is selected from an alkyl group having 3 to 7 carbon atoms.
[0057] In the liquid crystal / polymer composite material, by weight, there are 50.0 to 80.0 parts of mixed liquid crystal and 50.0 to 20.0 parts of ultraviolet light polymerizable monomer; the initiator and the gap particles account for 1 to 0.5 wt% and 0.2 to 0.5 wt% of the total mass of the mixed liquid crystal and the ultraviolet light polymerizable monomer, respectively; in the mixed liquid crystal, by weight, there are 62 to 24 parts of wide temperature range liquid crystal and 38 to 76 parts of low birefringence liquid crystal.
[0058] The present application is further described in detail below through examples.
[0059] In the following Examples 1-3 and Comparative Examples 1-2, the UV-polymerizable monomers used are compounds shown in Table 1.
[0060] Table 1 Compounds and ratios of UV-polymerizable monomers
[0061] name Proportion / % HA(Hexyl Acrylate) 18 DCPA (Dicyclopentadienyl Acrylate) 7 HDDA (Hexanediol Diacrylate) 5
[0062] In practical applications, the UV-polymerizable monomer can be selected as one of epoxy acrylate, polyurethane acrylate, polyester acrylate, polyene thiol system, polyether acrylate, or a mixture of multiple thereof, all of which can meet the technical requirements of this application and can be replaced with each other.
[0063] In the following Examples 1-3 and Comparative Examples 1-2, during UV polymerization, the photoinitiator used is trimethylbenzoyldiphenylphosphine oxide (TPO), and its structure is:
[0064]
[0065] In a specific embodiment, the photoinitiator of the present application may also be other photoinitiators capable of photopolymerizing ultraviolet light-polymerizable monomers, such as any one of benzoin ethyl ether, 2-hydroxy-2-methyl-1-phenylpropanone or benzoin diethyl ether.
[0066] In the following Examples 1-3 and Comparative Examples 1-2, the wide temperature range liquid crystal is selected from the high refractive index wide temperature range liquid crystal XP-6011 produced by Yantai Xianhua Technology Group Co., Ltd., and its technical indicators are: Δn=0.208, Δε=12.2, T Cr-N <-40℃,T I-N =119℃, viscosity=72mPa·s; low birefringence liquid crystal uses low refractive index wide temperature range liquid crystal XP-6018 produced by Yantai Xianhua Technology Group Co., Ltd., and its technical indicators are Δn=0.1, Δε=4, T Cr-N <-40℃,T I-N =126°C, viscosity = 38 mPa·s, which contains the above three liquid crystal compounds:
[0067]
[0068] Of course, in specific implementation, the wide temperature range liquid crystal of the present application can also be produced by other companies, as long as it has the characteristics defined in claim 1 of the present application.
[0069] In the following Examples 1-3 and Comparative Examples 1-2, the mixed liquid crystal is compounded by the wide temperature range liquid crystal and the low birefringence liquid crystal, and the ratio and physical parameters of the mixed liquid crystal are shown in Table 2. The numbers of the mixed liquid crystal are Y1, Y2, Y3, Y4, and Y5 as shown in Table 1.
[0070] Table 2 Composition and physical parameters of mixed liquid crystal
[0071] LC Composition (wt.%) Δn Δε <![CDATA[n o ]]> <![CDATA[ε ⊥ ]]> η(mPa·s) <![CDATA[T N-I (℃)]]> Y1 100% XP-6011 0.208 12.2 1.514 5.3 72 119.4 Y2 62%XP-6011+38%XP-6018 0.15 9.0 1.505 4.9 53 121.6 Y3 43%XP-6011+57%XP-6018 0.135 8.5 1.500 4.7 48 122.3 Y4 24%XP-6011+76%XP-6018 0.115 7.5 1.494 4.5 42 124.1 Y5 100% XP-6018 0.1 4.0 1.487 4.4 38 126.7
[0072] In the following Examples 1-3 and Comparative Examples 1-2, the particle size of the glass microbeads is 20.0 μm. The glass microbeads are used to control the film thickness of the liquid crystal / polymer composite material to be maintained at 10 to 20 μm, and the specific thickness can be selected according to actual needs.
[0073] Example 1
[0074] S1, add 38 parts of liquid crystal XP-6018 to 62 parts of liquid crystal XP-6011, heat and stir until transparent, and cool naturally to obtain a mixed liquid crystal, recorded as Y2; mix the ultraviolet light polymerizable monomers according to the mass fraction ratio in Table 1, and after fully stirring, obtain a colorless and transparent liquid at room temperature, marked as polymerizable mixed liquid A.
[0075] S2, mixing the liquid crystal Y2 and the prepared polymerizable mixed liquid A in a mass percentage of 7:3, adding a photoinitiator and glass beads respectively to 1wt% and 0.3wt% of the total mass of the mixed liquid crystal and the ultraviolet light polymerizable monomer, stirring at room temperature to form a uniform liquid for use.
[0076] S3, the mixed liquid of S2 is poured into the middle of the transparent conductive plastic film coated with indium tin oxide by roll-to-roll processing, and cured in a UV curing box at the same time. The curing condition is irradiation with ultraviolet light with a wavelength of 365nm and an intensity of 15mW / cm 2 , the curing temperature is 28°C, the time is 300s, and an electrically controlled liquid crystal dimming film with a wide temperature range is prepared, and the intermediate layer is recorded as film X1.
[0077] Example 2
[0078] S1, add 57 parts of liquid crystal XP-6018 to 43 parts of liquid crystal XP-6011, heat and stir until transparent, and cool naturally to obtain a mixed liquid crystal, recorded as Y3; mix the ultraviolet light polymerizable monomers according to the mass fraction ratio in Table 1, and after fully stirring, obtain a colorless and transparent liquid at room temperature, marked as polymerizable mixed liquid A.
[0079] S2, mixing the liquid crystal Y3 and the prepared polymerizable mixed liquid A in a mass percentage of 7:3, adding a photoinitiator and glass beads respectively to 1wt% and 0.3wt% of the total mass of the mixed liquid crystal and the ultraviolet light polymerizable monomer, stirring at room temperature to form a uniform liquid for use.
[0080] S3, the mixed liquid of S2 is poured into the middle of the transparent conductive plastic film coated with indium tin oxide by roll-to-roll processing, and cured in a UV curing box at the same time. The curing condition is irradiation with ultraviolet light with a wavelength of 365nm and an intensity of 15mW / cm2 , the curing temperature is 30°C, the time is 300s, and an electrically controlled liquid crystal dimming film with a wide temperature range is prepared, and the intermediate layer is recorded as film X2.
[0081] Example 3
[0082] S1, add 76 parts of liquid crystal XP-6018 to 24 parts of liquid crystal XP-6011, heat and stir until transparent, and cool naturally to obtain a mixed liquid crystal, recorded as Y4; mix the ultraviolet light polymerizable monomers according to the mass fraction ratio in Table 1, and after fully stirring, obtain a colorless and transparent liquid at room temperature, marked as polymerizable mixed liquid A.
[0083] S2, mix the liquid crystal Y4 and the prepared polymerizable mixed liquid A in a mass percentage of 7:3, add a photoinitiator and glass beads respectively to 1wt% and 0.3wt% of the total mass of the mixed liquid crystal and the ultraviolet light polymerizable monomer, stir at room temperature to form a uniform liquid, and set aside.
[0084] S3, the mixed liquid of S2 is poured into the middle of the transparent conductive plastic film coated with indium tin oxide by roll-to-roll processing, and cured in a UV curing box at the same time. The curing condition is irradiation with ultraviolet light with a wavelength of 365nm and an intensity of 15mW / cm 2 , the curing temperature is 28°C, the time is 300s, and an electrically controlled liquid crystal dimming film with a wide temperature range is prepared, and the intermediate layer is recorded as film X3.
[0085] Comparative Example 1
[0086] S1, take liquid crystal XP-6011, denoted as Y1; mix the ultraviolet light polymerizable monomers according to the mass fraction ratio in Table 1, and after fully stirring, obtain a colorless and transparent liquid at room temperature, marked as polymerizable mixed liquid A.
[0087] S2, mixing the liquid crystal Y1 and the prepared polymerizable mixed liquid A in a mass percentage of 7:3, adding a photoinitiator and glass beads respectively to 1wt% and 0.3wt% of the total mass of the mixed liquid crystal and the ultraviolet light polymerizable monomer, stirring at room temperature to form a uniform liquid for use.
[0088] S3, the mixed liquid of S2 is poured into the middle of the transparent conductive plastic film coated with indium tin oxide by roll-to-roll processing, and cured in a UV curing box at the same time. The curing condition is irradiation with ultraviolet light with a wavelength of 365nm and an intensity of 15mW / cm 2 , the curing temperature is 26°C, the time is 300s, and an electrically controlled liquid crystal dimming film with a wide temperature range is prepared, and the intermediate layer is recorded as film D1.
[0089] Comparative Example 2
[0090] S1, take liquid crystal XP-6018, denoted as Y5; mix the ultraviolet light polymerizable monomers according to the mass fraction ratio in Table 1, and after fully stirring, obtain a colorless and transparent liquid at room temperature, marked as polymerizable mixed liquid A.
[0091] S2, mix the liquid crystal Y5 and the prepared polymerizable mixed liquid A in a mass percentage of 7:3, add a photoinitiator and glass beads respectively to 1wt% and 0.3wt% of the total mass of the mixed liquid crystal and the ultraviolet light polymerizable monomer, stir at room temperature to form a uniform liquid, and set aside.
[0092] S3, the mixed liquid of S2 is poured into the middle of the transparent conductive plastic film coated with indium tin oxide by roll-to-roll processing, and cured in a UV curing box at the same time. The curing condition is irradiation with ultraviolet light with a wavelength of 365nm and an intensity of 15mW / cm 2 , the curing temperature is 26°C, the time is 300s, and an electrically controlled liquid crystal dimming film with a wide temperature range is prepared, and the intermediate layer is recorded as film D2.
[0093] The electro-optical properties of the dimming films X1-X3 of Examples 1-3 and the dimming films D1-D2 prepared in Comparative Examples 1-2 were tested at -40°C and 100°C using a liquid crystal comprehensive parameter meter, including the saturation voltage V sat , contrast CR, on-state response time t R , Off-state response time t D . See Table 3 for specific test data.
[0094] Table 3 Electro-optical performance data of dimming film
[0095]
[0096] From the test results, it can be seen that as the content of low refractive index wide temperature range liquid crystal XP-6018 in the mixed liquid crystal increases, the contrast of the dimming film decreases accordingly. The dimming film D2 of comparative example 2, whose mixed liquid crystal only contains low refractive index wide temperature range liquid crystal XP-6018, has a contrast ratio of 4 at 100°C and a contrast ratio of 20 at -40°C, which are much lower than the dimming films X1, X2 and X3 of Examples 1-3. The low contrast ratio causes the dimming film D2 to still have a certain degree of transmittance when it is not turned on, which reduces the privacy protection function of the dimming film.
[0097] Saturation voltage V of dimming films X1, X2 and X3 sat , Open state response time t R , Off-state response time t D , which is similar to the dimming film D1 of comparative example 1 and the dimming film D2 of comparative example 2, has excellent high temperature performance, and also has a lower saturation voltage and a faster response time at -40°C.
[0098] The dimming films X1-X3 of Examples 1-3 and the dimming films D1-D2 prepared in Comparative Examples 1-2 were cut into 2cm*3cm small pieces, placed on a shelf, and an applied voltage of 60V was used. The incident light was perpendicular to the sample film at 0°, and the sample film was photographed at ±60° to observe the actual state. The open-state light transmittance of each dimming film from 0° to 60° and the open-state haze at 0° and 60° were tested. The incident laser for the test was a 590nm He-Ne laser with a maximum voltage of 100V and a frequency of 1000Hz. The air transmittance was normalized to 100%. The curve of the test data is shown in Figures 1 to 10 , see the actual picture Fig.11 , the test data are shown in Table 4.
[0099] Table 4 Transmittance and haze data of dimming film
[0100] Transmittance 0°(%) Transmittance 60°(%) Haze 0°(%) Haze 60°(%) D1 81.2 38.2 5.3 31.5 D2 82.3 70.5 2.8 10.5 X1 81.4 55.6 3.1 19.6 X2 82.5 62.5 2.4 14.8 X3 83.5 71.5 2.5 11.9
[0101] Depend on Figure 1-Figure 10 From the test data curve graph and the test data in Table 4, it can be seen that the dimming films X1-X3 of Examples 1-3 can reach up to 71.5% when the observation angle is 60°; the dimming films of Examples 1-3 have a haze of 11.9-19.6% when the observation angle is 60°. However, the transmittance of the dimming film D1 of Comparative Example 1 is only 38.2% when the observation angle is 60°, and the haze is as high as 31.5%. When the observation angle is 60°, the haze of the dimming films X1-X3 of Examples 1-3 is much lower than that of the dimming film D1 of Comparative Example 1, while the transmittance is much higher than that of the dimming film D1 of Comparative Example 1. The dimming film X3 of Example 3 has the best comprehensive performance.
[0102] The dimming film D2 of comparative example 2 has a haze lower than the dimming films X1-X3 of embodiments 1-3 at an observation angle of 60°; and its haze is comparable to the dimming films X1-X3 of embodiments 1-3 at an observation angle of 0°. However, the contrast of the dimming film D2 of comparative example 2 is much lower than that of the dimming films X1-X3 of embodiments 1-3, resulting in it still being semi-transparent when not powered on. Fig.11 As shown, the dimming film D2 of comparative example 2 loses its light regulating function and is not suitable for practical applications.
[0103] Within the ratio range of the mixed liquid crystal of the present application, the dimming films X1-X3 prepared in Examples 1-3 have a large viewing angle and low off-axis haze while having a high contrast ratio.
[0104] Example 4
[0105] S1, add 76 parts of liquid crystal XP-6018 to 24 parts of liquid crystal XP-6011, heat and stir until transparent, and cool naturally to obtain a mixed liquid crystal, recorded as Y4; mix the ultraviolet light polymerizable monomers according to the mass fraction ratio in Table 1, and after fully stirring, obtain a colorless and transparent liquid at room temperature, marked as polymerizable mixed liquid A.
[0106] S2, mix the liquid crystal Y4 and the prepared polymerizable mixed liquid A in a mass percentage of 5:5, add a photoinitiator and glass beads respectively to 0.5wt% and 0.2wt% of the total mass of the mixed liquid crystal and the ultraviolet light polymerizable monomer, and stir at room temperature to form a uniform liquid for use.
[0107] S3, the mixed liquid of S2 is poured into the middle of the transparent conductive plastic film coated with indium tin oxide by roll-to-roll processing, and cured in a UV curing box at the same time. The curing condition is irradiation with ultraviolet light with a wavelength of 365nm and an intensity of 30mW / cm 2 , the curing temperature is 28℃, the curing time is 100s, and the electrically controlled liquid crystal dimming film X4 with a wide temperature range is prepared, and the interlayer is recorded as film X4. The electro-optical performance of dimming film X4 is similar to that of dimming film X3, both of which have high contrast at high temperature, and also show a low saturation voltage at -40℃, while maintaining a low off-axis haze.
[0108] Example 5
[0109] S1, add 76 parts of liquid crystal XP-6018 to 24 parts of liquid crystal XP-6011, heat and stir until transparent, and cool naturally to obtain a mixed liquid crystal, recorded as Y4; mix the ultraviolet light polymerizable monomers according to the mass fraction ratio in Table 1, and after fully stirring, obtain a colorless and transparent liquid at room temperature, marked as polymerizable mixed liquid A.
[0110] S2, mix the liquid crystal Y4 and the prepared polymerizable mixed liquid A in a mass percentage of 8:2, add a photoinitiator and glass beads respectively to 0.5wt% and 0.5wt% of the total mass of the mixed liquid crystal and the ultraviolet light polymerizable monomer, and stir at room temperature to form a uniform liquid for use.
[0111] S3, the mixed liquid of S2 is poured into the middle of the transparent conductive plastic film coated with indium tin oxide by roll-to-roll processing, and cured in a UV curing box at the same time. The curing condition is irradiation with ultraviolet light with a wavelength of 365nm and an intensity of 30mW / cm 2, the curing temperature is 28℃, the curing time is 100s, and the electrically controlled liquid crystal dimming film X5 with a wide temperature range is prepared, and the interlayer is recorded as film X5. The electro-optical performance of dimming film X5 is similar to that of dimming film X3, both of which have high contrast at high temperature, and also show a low saturation voltage at -40℃, while maintaining a low off-axis haze.
[0112] Example 6
[0113] The preparation method of this embodiment is the same as that of Example 3, except that the UV light polymerizable monomer is any one of epoxy acrylate, polyurethane acrylate, polyester acrylate, epoxy acrylate, polyene thiol system, polyether acrylate, and vinyl ether, and the other process parameters remain unchanged. The electro-optical performance of the obtained electrically-controlled dimming film is close to that of the dimming film X3, and both have high contrast at high temperature. At the same time, it also shows a low saturation voltage at minus 40°C, while maintaining a low off-axis haze.
[0114] Example 7
[0115] The preparation method of this embodiment is the same as that of embodiment 3, except that the wide temperature range liquid crystal is replaced by XP-6015 (technical indicators: Δn=0.250, TCr-N<-40°C, T I-N =122℃, viscosity (100kPa, 20℃) = 107mPa·s), and the other process parameters and materials remain unchanged. The electro-optical performance of the obtained electrically-controlled dimming film is close to that of the dimming film X4. Both have high contrast at high temperatures and show low saturation voltage at -40℃, while maintaining low off-axis haze.
[0116] The wide temperature range dimming film with low off-axis haze prepared in this application has the characteristics of large viewing angle and low off-axis haze. When applied to car windows, it can maintain a good field of view and improve the comfort of drivers and passengers as well as driving safety. The wide temperature range dimming film with low off-axis haze prepared in this application is applied to building windows. It has good privacy in the disconnected state and good field of view in the connected state, which improves the comfort of people in the building.
[0117] Although the present application has been described in detail in general terms and in specific embodiments in this specification, it is obvious to those skilled in the art that some modifications or improvements may be made to the present application. Therefore, these modifications or improvements made without departing from the spirit of the present application are within the scope of protection claimed in the present application.
Claims
1. A wide temperature range dimming film with low off-axis haze, characterized in that: It comprises three layers, namely, upper, middle and lower layers, which are stacked in layers along the thickness direction, wherein the upper and lower layers are conductive glass or conductive plastic film, and the middle layer is a liquid crystal / polymer composite material, wherein the liquid crystal / polymer composite material comprises a mixed liquid crystal, an ultraviolet light polymerizable monomer, a photoinitiator and interstitial particles; The mixed liquid crystal has a birefringence greater than 0.1 and less than 0.15, a crystallization point less than -40°C, a clearing point greater than 120°C, a viscosity less than 80 mPas, and a dielectric anisotropy greater than 3.
2. The low off-axis haze wide temperature range dimming film according to claim 1, characterized in that: The mixed liquid crystal includes a wide temperature range liquid crystal and a low birefringence liquid crystal; The wide temperature range liquid crystal is a nematic phase liquid crystal, with a birefringence greater than 0.18, a crystallization point less than -40°C, a clearing point greater than 120°C, and a viscosity less than 80 mPas; The low birefringence liquid crystal is a positive nematic phase liquid crystal, and its birefringence is ≤0.1; In the mixed liquid crystal, the wide temperature range liquid crystal accounts for 62 to 24 parts, and the low birefringence liquid crystal accounts for 38 to 76 parts by weight.
3. The low off-axis haze wide temperature range dimming film according to claim 2, characterized in that: The low birefringence liquid crystal comprises the following compounds: ; ; ; Wherein, R1 and R2 are groups -F or -CN, and R3 is selected from an alkyl group having 3 to 7 carbon atoms.
4. The low off-axis haze wide temperature range dimming film according to claim 1, characterized in that: The liquid crystal / polymer composite material comprises, by weight, 50.0 to 80.0 parts of mixed liquid crystal and 50.0 to 20.0 parts of ultraviolet light polymerizable monomer; The initiator and the gap particles account for 1-0.5 wt% and 0.2-0.5 wt% of the total mass of the mixed liquid crystal and the ultraviolet light polymerizable monomer respectively.
5. The low off-axis haze wide temperature range dimming film according to claim 1, characterized in that: The ultraviolet light polymerizable monomer is any one or more of epoxy acrylate, polyurethane acrylate, polyester acrylate, epoxy acrylate, polyene thiol system, polyether acrylate and vinyl ether.
6. The low off-axis haze wide temperature range dimming film according to claim 1, characterized in that: The photoinitiator is at least one of benzoin ethyl ether, 2-hydroxy-2-methyl-1-phenylacetone, trimethylbenzoyl diphenyl phosphine oxide, and benzoin diethyl ether.
7. The low off-axis haze wide temperature range dimming film according to claim 1, characterized in that: The thickness of the liquid crystal / polymer composite material is 10-20 μm, and the diameter of the gap particles is 10-20 μm.
8. Use of the low off-axis haze and wide temperature range dimming film according to any one of claims 1 to 7 in automobile windows or building windows.