A double active layer terbium doped oxide thin film transistor and its preparation method

By using two terbium-doped oxide films with different terbium element contents to construct a dual active layer channel in the TFT, the low carrier mobility and instability of traditional InGaZnO TFTs under negative bias light illumination stress is solved. , high mobility and high stability oxide TFT is achieved, reducing the manufacturing cost of AMOLED display.

CN117457753BActive Publication Date: 2024-11-19ZHANGZHOU HEQI TARGET TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311546351.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-20
Publication Date
2024-11-19
Estimated Expiration
2043-11-20

AI Technical Summary

Technical Problem

The carrier mobility of traditional InGaZnO TFTs under negative bias light illumination stress is low and unstable, resulting in negative drift of threshold voltage, increasing the manufacturing cost of AMOLED display.

Method used

Two terbium-doped oxide films with different terbium contents are used to construct a dual active layer channel. The high terbium-doped oxide films are used as the top channel layer to suppress photoionization of oxygen vacancies and reduce water oxygen. The influence of adsorption on carrier transport improves the carrier mobility and stability of TFT.

Benefits of technology

High mobility and high stability oxide TFT is achieved, carrier mobility reaches 40 cm2/Vs, switching current ratio is higher than 108, and threshold voltage negative drift is less than 1 V per hour, reducing manufacturing cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117457753B_ABST
    Figure CN117457753B_ABST
Patent Text Reader

Abstract

The present invention provides a double active layer oxide thin film transistor with good NBIS stability and a preparation method thereof, wherein the thin film transistor comprises a first active layer and a second active layer, wherein the terbium content of the first active layer thin film is less than that of the second active layer thin film. The present invention gives full play to the characteristics of high oxygen binding energy and low charge transfer transition energy of terbium, improves the electrical performance and stability of the oxide thin film transistor by doping a small amount of terbium, constructs a double active layer channel by stacking two layers of oxide semiconductor thin films with different terbium content layer by layer, and improves the carrier mobility and stability of the oxide TFT by precisely controlling the active layer oxide semiconductor thin film material components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of microelectronic technology, specifically relates to semiconductor technology, and in particular to a double-active-layer terbium-doped oxide transistor with good negative bias illumination stress (NBIS) and a preparation method thereof. Background Art

[0002] As the core device of display driver, thin film transistor (TFT) has always received extensive attention. Among the backplane driver technologies that have been commercialized, the field effect mobility of amorphous silicon TFT is low and cannot meet the needs of new display drivers. Oxide TFT has high mobility, good large-area uniformity and extremely low off-state current, providing support for new high-resolution and low-power display technologies.

[0003] Traditional InGaZnO TFTs require a large amount of Ga doping to suppress the carrier concentration in the semiconductor and adjust the threshold voltage. However, due to the large difference in radius between Ga ions and In ions, a large amount of Ga doping will affect the overlap of the 5s electron orbits of In ions, resulting in a serious reduction in TFT carrier mobility. More importantly, oxide TFTs will experience severe threshold voltage negative drift and even increased subthreshold swing under the action of continuous negative bias illumination stress (NBIS), and will not recover within a few days after the bias stress is removed. This directly leads to an increase in the difficulty of designing compensation circuits in the TFT driver backplane, increasing the manufacturing cost of AMOLED displays.

[0004] Therefore, how to improve the carrier mobility and NBIS stability of oxide TFTs has become a problem that needs to be solved urgently. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a dual active layer oxide thin film transistor and a method for preparing the same. The dual active layer oxide thin film transistor prepared according to the present invention has the advantages of high mobility, high stability and the like.

[0006] The present invention uses two layers of terbium-doped oxide films with different terbium content to construct a dual active layer channel to improve the carrier mobility of the oxide TFT device. Specifically, a terbium-doped oxide film with a high terbium content is used as the top channel layer to suppress the photoionization of oxygen vacancies in the active layer under NBIS, while reducing the influence of external water and oxygen adsorption on the bottom channel layer of high-speed carrier transmission, thereby improving the NBIS stability of the TFT device, and thus realizing an oxide TFT with high mobility and high stability.

[0007] The above-mentioned purpose of the present invention is achieved by the following technical means:

[0008] In a first aspect, the present invention provides a dual-active layer oxide thin film transistor, comprising a first active layer and a second active layer, wherein the terbium content of the oxide semiconductor thin film of the first active layer is 0 at% to 5 at%; the terbium content of the oxide semiconductor thin film of the second active layer is 5 at% to 15at%, and the terbium content of the first active layer thin film is less than the terbium content of the second active layer thin film.

[0009] Preferably, the double active layer oxide thin film transistor is provided with a substrate, a gate electrode, a gate insulating layer, a first active layer, a second active layer and a source / drain electrode in sequence.

[0010] Preferably, the terbium-doped oxide semiconductor film composition in the first active layer and / or the second active layer includes (InO) x (MO) y (TbO) z , wherein the terbium element exists in the form of a trivalent ion, a tetravalent ion or a mixed valence state.

[0011] Preferably, the Tb content of the first active layer is 3 at%.

[0012] Preferably, the Tb content of the second active layer is 10 at%

[0013] Preferably, M is an element selected from the group consisting of Li, Zn and Sn or a combination of any two of them.

[0014] Preferably, the first active layer is a bottom channel layer, and the second active layer is a top channel layer.

[0015] Preferably, the thickness of the oxide semiconductor film of the first active layer is 2 nm to 20 nm; the thickness of the oxide semiconductor film of the second active layer is 5 nm to 50 nm.

[0016] Preferably, the thickness of the first active layer film is smaller than the thickness of the second active layer film.

[0017] Preferably, the carrier mobility of the dual active layer oxide thin film transistor is as high as 40 cm 2 / Vs, the switching current ratio is higher than 10 8 , the negative drift value of the threshold voltage under the action of NBIS is less than 1V per hour.

[0018] Preferably, the film is prepared by a vacuum method, including but not limited to sputtering, pulsed laser deposition, atomic layer deposition, and chemical vapor deposition.

[0019] Preferably, the film is prepared by a solution method, including but not limited to spin coating, inkjet printing, screen printing, doctor blade coating, and embossing.

[0020] On the other hand, the present invention also provides a method for preparing a dual active layer oxide thin film transistor, the preparation method specifically comprising:

[0021] Step S1: preparing a gate electrode and a gate insulating layer on the surface of a substrate;

[0022] Step S2: preparation of precursor solution;

[0023] Step S3: preparing a first active layer on a surface of the gate insulating layer away from the substrate, and preparing a second active layer on a surface of the first active layer;

[0024] Step S4: preparing source and drain electrodes to obtain a TFT device;

[0025] The terbium content of the first active layer thin film is less than that of the second active layer thin film; the preparation of the precursor solution in step S2 can be placed in any step before use.

[0026] Preferably, step S2 includes preparing the first active layer and / or the second active layer by a solution method or a vacuum method.

[0027] Preferably, step S1 includes: preparing one or more conductive films by physical vapor deposition, and patterning them by hollow mask or photolithography to obtain a gate electrode; preparing an insulating layer by anodization, thermal oxidation, physical vapor deposition or chemical vapor deposition, and patterning them by hollow mask or photolithography.

[0028] Preferably, one or more conductive films are prepared by vacuum evaporation or sputtering, and patterned by hollow mask or photolithography to obtain source and drain electrodes.

[0029] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0030] The present invention provides a high-mobility, high-stability dual-active-layer Tb-doped oxide thin-film transistor and a preparation method thereof. The dual-active-layer Tb-doped oxide thin-film transistor prepared by the present invention fully utilizes the characteristics of high oxygen binding energy and low charge transfer transition energy of terbium ions, and improves the electrical bias stability of the device by doping a small amount of terbium element.

[0031] The present invention uses two layers of terbium-doped oxide films with different terbium content and film thickness to stack layer by layer to construct a double active layer channel, wherein the terbium-doped oxide film with low terbium content and low film thickness is used as the bottom channel layer, and the terbium-doped oxide film with high terbium content and high film thickness is used as the top channel layer. By accurately controlling the channel layer material composition and film thickness, the carrier mobility and stability of the oxide TFT are improved.

[0032] The present invention adopts a terbium-doped oxide film with a high terbium content as a top channel layer, suppresses the photoionization of oxygen vacancies in the active layer under NBIS, and reduces the influence of external water and oxygen adsorption on the bottom channel layer of high-speed carrier transmission, thereby improving the NBIS stability of the TFT device, and further realizing an oxide TFT with high mobility and high stability.

[0033] The double active layer terbium-doped oxide thin film transistor prepared by the method of the present invention has a carrier mobility of up to 40cm 2 / Vs, switch current ratio higher than 10 8 , and the negative drift value of the threshold voltage under the action of NBIS is less than 1 V per hour.

[0034] The preparation method of the present invention directly adopts the sol-gel method, has simple process, low requirements on experimental conditions, high controllability, low cost, can be mass-produced over a large area, has high repeatability, and meets environmental requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 A schematic structural diagram of a double active layer oxide thin film transistor device with good NBIS stability prepared by the present invention;

[0036] Figure 2 is a transfer characteristic curve of a double active layer terbium-doped oxide thin film transistor provided in the first embodiment of the present invention;

[0037] Figure 3 is a transfer characteristic curve of a single active layer terbium-doped oxide thin film transistor prepared in Comparative Example 1 of the present invention;

[0038] Figure 4 is a transfer characteristic curve of a single active layer terbium-doped oxide thin film transistor prepared in Comparative Example 2 of the present invention;

[0039] Figure 5 It is the drift of the device threshold voltage with the stress action time under the action of NBIS (a) and PBIS (b) of the double active layer terbium-doped oxide thin film transistor prepared in Example 1 of the present invention and the single active layer prepared in the comparative example;

[0040] Figure 6 is a transfer characteristic curve of a double active layer terbium-doped oxide thin film transistor prepared in Example 2 of the present invention;

[0041] Figure 7 This is a transfer characteristic curve of the double active layer terbium-doped oxide thin film transistor prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0042] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention. It should also be noted that, for ease of description, only parts related to the present invention, rather than all structures, are shown in the accompanying drawings.

[0043] Embodiment 1

[0044] Figure 1 A schematic structural diagram of a TFT device with good NBIS stability obtained by a method for preparing a double active layer oxide thin film transistor provided by the present invention.

[0045] The schematic cross-sectional diagram of the dual active layer oxide thin film transistor is as follows: Figure 1 As shown, a substrate 10, a gate electrode 11, a gate insulating layer 12, a first active layer 13, a second active layer 14, a source electrode 15a and a drain electrode 15b are sequentially arranged.

[0046] Embodiment 1 of the present invention provides a method for preparing a dual active layer oxide thin film transistor with good NBIS stability, the method comprising:

[0047] Step S1: preparing a gate electrode 11 and a gate insulating layer 12 on the surface of a substrate 10 .

[0048] Wherein, step S1 specifically includes:

[0049] Step S11 : depositing a metal film as the gate electrode 11 on the surface of the cleaned substrate 10 by vacuum physical vapor deposition.

[0050] Preferably, the metal film is an Al metal film, which is patterned by ultraviolet lithography or wet etching.

[0051] Step S12 : depositing a gate insulating layer 12 on the surface of the gate electrode 11 .

[0052] Preferably, an oxide is formed as an insulating layer by anodization, and ultraviolet light or plasma is used for surface treatment; the anodized substrate is ultrasonically cleaned in deionized water and isopropanol for 10 minutes, respectively, and dried in an oven at 70° C., and then irradiated under ultraviolet light for 30 minutes.

[0053] Step S2: Preparation of precursor solution.

[0054] Metal salts of indium and terbium are selected as precursors, mixed and dissolved in deionized water or an organic solvent, stirred at room temperature, and filtered before use.

[0055] The total molar concentration of all metal cations was controlled to be 0.01-0.5 mol / L, and different metal cations were mixed in specific proportions and marked separately. The solution with low molar concentration and low terbium ion content was marked as solution A, and the solution with high molar concentration and high terbium ion content was marked as solution B.

[0056] Preferably, the step of "stirring at room temperature and filtering before use" is specifically stirring vigorously at room temperature for 12 hours and filtering through a 0.22 μm filter head before use.

[0057] Specifically, in this embodiment, solution A uses 0.551 g of indium nitrate hydrate (In(NO 3 ) 3 ·nH 2 O, 0.0085g lithium nitrate hydrate LiNO 3 ·nH 2 O and 0.026 g of terbium nitrate hydrate Tb(NO 3 ) 3 ·nH 2 O was dissolved in 10 mL of deionized water to obtain a precursor solution with a total cation molar concentration of 0.2 mol / L and an In:Li:Tb ion ratio of 92:5:3.

[0058] Solution B uses 0.770 g of indium nitrate hydrate (In(NO 3 ) 3 nH2O, 0.026 g lithium nitrate hydrate LiNO 3 nH2O and 0.131 g of terbium nitrate hydrate Tb(NO 3 ) 3 nH2O was dissolved in 10 mL of deionized water to obtain a precursor solution with a total cation molar concentration of 0.3 mol / L and an In:Li:Tb ion ratio of 85:5:10.

[0059] It is worth noting that the preparation step of the precursor solution belongs to the preparatory step, which can be placed in any step before use.

[0060] Step S3 : preparing a first active layer 13 on a surface of the gate insulating layer 12 away from the substrate 10 , and preparing a second active layer 14 on a surface of the first active layer 13 .

[0061] Wherein, step S3 specifically includes:

[0062] Step S31: pre-grow solution A on the surface of the gate insulating layer 12 by solution processing, control the molar concentration of the solution to obtain a desired thickness, and perform annealing in an atmospheric environment to obtain a terbium-doped oxide thin film as the first active layer 13.

[0063] Preferably, the oxide semiconductor film of the first active layer has a thickness of 5 nm.

[0064] Step S32: using ultraviolet light or plasma to perform surface treatment on the first active layer 13 .

[0065] Specifically, oxygen plasma cleaning (O-plasma) is used to perform surface treatment on the first active layer 13, with a power of 100 W and a time of 60 s.

[0066] Step S33: pre-grow solution B on the surface of the first active layer 13 by solution processing, control the solution molar concentration to obtain the desired thickness, perform annealing in an atmospheric environment to obtain a terbium-doped oxide film to obtain the second active layer 14, and pattern the dual active layer channel by ultraviolet lithography or wet etching.

[0067] Preferably, the solution B is pre-grown on the first active layer 13 by spin coating to obtain the second active layer 14 .

[0068] Preferably, the oxide semiconductor film thickness of the second active layer is 7 nm.

[0069] Furthermore, the precursor solvent may be deionized water, ethylene glycol, ethylene glycol monomethyl ether or a mixed solution thereof, and the concentration of the precursor solution is 0.01-0.3 mol / L.

[0070] The solution processing technology is spin coating, spray coating, or inkjet printing; the annealing treatment method is photon sintering, laser annealing, microwave heating annealing, or ordinary thermal annealing, and the annealing temperature is 150°C to 500°C.

[0071] Preferably, the first active layer 13 is a bottom channel layer, and the second active layer 14 is a top channel layer.

[0072] Step S4: Prepare source and drain electrodes to obtain a TFT device.

[0073] A TFT device was obtained by evaporating 80 nm thick Al as source and drain electrodes on the double active layer using a mask patterning method.

[0074] The transfer characteristic curve of the double active layer terbium-doped oxide thin film transistor in this embodiment is obtained through testing as follows: Figure 2As shown, the horizontal axis is the gate voltage and the vertical axis is the source / drain current; the curve test condition is the source / drain voltage V DS =15.1V, gate scan voltage V GS =-30~30V.

[0075] The test results show that the carrier mobility of the double active layer terbium-doped oxide thin film transistor provided by the present invention is as high as 40 cm 2 / Vs, switch current ratio higher than 10 8 , the threshold voltage is close to 0 V, NBIS (negative bias illumination stress) and PBIS (positive bias illumination stress) are stable, and the threshold voltage change is less than 1 V per hour.

[0076] In order to demonstrate the advantages of the dual active layer oxide thin film transistor provided by the present invention in terms of performance improvement, the present invention also provides two comparative examples (Comparative Example 1 and Comparative Example 2) for comparing the electrical properties of the dual active layer terbium-doped oxide thin film transistor, which respectively use the same precursor solution (A or B) and preparation process as the embodiments of the present invention to prepare a single active layer terbium-doped oxide thin film transistor.

[0077] Comparative Example 1

[0078] The present invention also provides a single active layer terbium-doped oxide thin film transistor as comparative example 1. The specific preparation method of the single active layer terbium-doped oxide thin film transistor is:

[0079] (1) Preparation of precursor solution: Solution A uses a certain amount of indium nitrate hydrate (In(NO 3 ) 3 ·nH 2 O, Lithium nitrate hydrate LiNO 3 ·nH 2 O and terbium nitrate hydrate Tb(NO 3 ) 3 ·nH 2 O was dissolved in deionized water to obtain a precursor solution with a total cation molar concentration of 0.2 mol / L, in which the In:Li:Tb ion ratio was 92:5:3. All solutions were stirred vigorously at room temperature for 12 hours and filtered through a 0.22 μm filter before use.

[0080] (2) A layer of Al metal film is deposited on the cleaned glass surface by vacuum physical vapor deposition as a gate electrode and patterned by photolithography. Then, anodization is performed to form an oxide as an insulating layer.

[0081] (3) The anodized substrate was ultrasonically cleaned in deionized water and isopropanol for 10 minutes, respectively, and dried in an oven at 70°C. It was then irradiated under ultraviolet light for 30 minutes.

[0082] Solution A is pre-grown on the gate insulating layer by spin coating, and then annealed in an atmospheric environment to obtain a terbium-doped oxide film as a single channel layer. The single active layer channel is patterned by ultraviolet lithography and wet etching.

[0083] (4) Using a mask patterning method, 80 nm thick Al was evaporated on the double active layer as source and drain electrodes to obtain a TFT device.

[0084] The transfer characteristic curve of the single active layer thin film transistor doped with 3 at% Tb is obtained through testing. Figure 3 As shown, Figure 3 As shown, the horizontal axis is the gate voltage and the vertical axis is the source / drain current; the curve test condition is the source / drain voltage V DS =15.1V, gate scan voltage V GS =-30~30V. Compared with the double active layer terbium doped oxide thin film transistor, the carrier mobility of the single active layer terbium doped oxide thin film transistor is 19 cm 2 / Vs, it can be seen that the single active layer terbium-doped oxide thin film transistor has low mobility and worse stability.

[0085] Comparative Example 2

[0086] As a single active layer terbium-doped oxide thin film transistor of comparative example 2, the specific preparation method of the single active layer terbium-doped oxide thin film transistor is:

[0087] (1) Preparation of precursor solution: Solution B uses 0.770 g of indium nitrate hydrate (In(NO 3 ) 3 ·nH 2 O, 0.026g lithium nitrate hydrate LiNO 3 ·nH 2 O and 0.131 g terbium nitrate hydrate Tb(NO 3 ) 3 ·nH 2O was dissolved in 10 mL of deionized water to obtain a precursor solution with a total cation molar concentration of 0.3 mol / L and an In:Li:Tb ion ratio of 85:5:10. All solutions were stirred vigorously at room temperature for 12 hours and filtered through a 0.22 μm filter before use.

[0088] (2) A layer of Al metal film is deposited on the cleaned glass surface by vacuum physical vapor deposition as a gate electrode and patterned by photolithography. Then, anodization is performed to form an oxide as an insulating layer.

[0089] (3) The anodized substrate was ultrasonically cleaned in deionized water and isopropanol for 10 minutes, respectively, and dried in an oven at 70°C. After that, it was irradiated with ultraviolet light for 30 minutes. Solution B was pre-grown on the gate insulating layer by spin coating, and then annealed in an atmospheric environment to obtain a terbium-doped oxide film as a single channel layer. The single active layer channel was patterned using ultraviolet lithography technology and wet etching.

[0090] (4) Using a mask patterning method, 80 nm thick Al was evaporated on the double active layer as source and drain electrodes to obtain a TFT device.

[0091] The transfer characteristic curve of the single active layer thin film transistor doped with 10 at% Tb is shown in the figure below: Figure 4 As shown, Figure 4 As shown, the horizontal axis is the gate voltage and the vertical axis is the source / drain current; the curve test condition is the source / drain voltage V DS =15.1V, gate scan voltage V GS =-30~30V.

[0092] Compared with the double active layer terbium-doped oxide thin film transistor, the carrier mobility of the single active layer terbium-doped oxide thin film transistor is 1.7 cm 2 / Vs, the mobility of the single active layer terbium-doped oxide thin film transistor is significantly lower.

[0093] For better comparison, the present invention provides a performance comparison diagram of a double active layer terbium-doped oxide thin film transistor and a single active layer terbium-doped oxide thin film transistor.

[0094] Figure 5 The drift of the threshold voltage of the device under NBIS (a) and PBIS (b) of the double active layer terbium-doped oxide thin film transistor prepared in Example 1 of the present invention and the single active layer terbium-doped oxide thin film transistor prepared in the comparative example with the stress action time, wherein the horizontal axis is the duration of the applied stress and the vertical axis is the threshold voltage change; the curve test condition is the source / drain voltage V DS=0.1V, gate voltage V GS =-20 V, light intensity is 1000 Lux.

[0095] It can be seen from Comparative Examples 1 and 2 that, in a single active layer terbium-doped oxide thin film transistor, a low terbium-doped device has a relatively high mobility, but poor NBIS stability.

[0096] With the increase of terbium doping concentration in the active layer, the threshold voltage of the single active layer terbium-doped oxide thin film transistor moves forward but the mobility decreases significantly, indicating that terbium doping can effectively suppress the electron concentration in the oxide semiconductor. At the same time, the NBIS stability of the device is significantly improved, that is, the threshold voltage change value of the device under NBIS is smaller, such as Figure 5 (a); However, high terbium doping concentration will lead to an increase in the interface defects of the insulating layer / active layer, making the PBIS stability of the device worse, that is, the threshold voltage change of the device under the action of PBIS is larger, such as Figure 5 (b). Therefore, in a single active layer terbium-doped oxide thin film transistor, there is an obvious restrictive relationship between the mobility and stability of the device.

[0097] In contrast, the double active layer terbium-doped oxide thin film transistor prepared by the same process in Example 1 has higher electron mobility and better NBIS and PBIS stability. Among them, the first active layer 13 with low terbium doping concentration can provide a good insulating layer / active layer interface and a high-speed electron transport path, achieving high PBIS stability and high electron mobility; the second active layer 14 with high terbium doping concentration can increase the overall terbium content of the active layer, promote the charge transfer transition of terbium ions and isolate water and oxygen adsorption, and achieve high NBIS stability. The good interface characteristics of the first active layer and the second active layer promote the aggregation of electrons and further improve the electron mobility of the device.

[0098] It can be seen that the present invention uses two layers of terbium-doped oxide films with different terbium content to stack layer by layer to construct a double active layer channel, thereby improving the carrier mobility and stability of the oxide TFT device.

[0099] The measurement results show that the carrier mobility of the double active layer terbium-doped oxide thin film transistor provided by the present invention is as high as 40 cm 2 / Vs, switch current ratio higher than 10 8 , the threshold voltage is close to 0 V, NBIS and PBIS have good stability, and the threshold voltage change under the action of NBIS and PBIS is less than 1 V per hour.

[0100] From the above, it can be seen that the double active layer terbium doped oxide thin film transistor has high electron mobility, large on-state current and low off-state current, and can achieve a high switching current ratio, a threshold voltage close to 0 V and a subthreshold swing of 0.3V / dec, indicating that the double active layer terbium doped oxide channel has good interface characteristics and low defect state density.

[0101] Embodiment 2

[0102] Embodiment 2 of the present invention provides a method for preparing a high-mobility and high-stability dual-active-layer terbium-doped oxide thin-film transistor, the method comprising:

[0103] Step S1: Precursor solution preparation.

[0104] In this embodiment, solution A uses a certain amount of indium nitrate hydrate (In(NO 3 ) 3 ·nH 2 O, Lithium nitrate hydrate LiNO 3 ·nH 2 O and terbium nitrate hydrate Tb(NO 3 ) 3 ·nH 2 O was dissolved in deionized water to obtain a precursor solution with a total cation molar concentration of 0.2 mol / L and an In:Li:Tb ion ratio of 95:5:0.

[0105] Solution B uses a certain amount of indium nitrate hydrate In(NO 3 ) 3 ·nH 2 O, Lithium nitrate hydrate LiNO 3 ·nH 2 O and terbium nitrate hydrate Tb(NO 3 ) 3 ·nH 2 O was dissolved in deionized water to obtain a precursor solution with a total cation molar concentration of 0.3 mol / L and an In:Li:Tb ion ratio of 85:5:10. All solutions were stirred vigorously at room temperature for 12 hours and filtered through a 0.22 μm filter before use.

[0106] Step S2: depositing a layer of Al metal film as the gate electrode 11 on the surface of the cleaned glass substrate 10 by vacuum physical vapor deposition, and patterning by photolithography, and then forming an oxide as the gate insulating layer 12 by anodization.

[0107] Step S3: The anodized substrate was ultrasonically cleaned in deionized water and isopropanol for 10 minutes respectively, dried in an oven at 70° C., and then irradiated under ultraviolet light for 30 minutes.

[0108] Step S4: pre-grow solution A on the surface of the gate insulating layer 12 away from the substrate 10 by spin coating, and then perform annealing treatment in an atmospheric environment to obtain a first active layer 13 .

[0109] The film thickness was 5 nm by controlling the molar concentration of the solution.

[0110] Step S5: using oxygen plasma to perform surface treatment on the first active layer 13 at a power of 100 W for 60 seconds.

[0111] Step S6: pre-grow solution B on the first active layer 13 by spin coating, and then perform annealing treatment in an atmospheric environment to obtain the second active layer 14.

[0112] The thickness of the film was obtained to be 7 nm by controlling the molar concentration of the solution, and the dual active layer channel was patterned using UV lithography and wet etching.

[0113] Step S7: using a mask patterning method to evaporate 80 nm thick Al on the double active layer as source and drain electrodes to obtain a TFT device.

[0114] The transfer characteristic curve of the double active layer terbium-doped oxide thin film transistor in this embodiment is obtained through testing as follows: Figure 6 As shown, the horizontal axis is the gate voltage and the vertical axis is the source / drain current; the curve test condition is the source / drain voltage V DS =15.1V, gate scan voltage V GS =-30~30V.

[0115] According to the experimental results, the carrier mobility of the double active layer terbium-doped oxide thin film transistor provided by the present invention is as high as 47 cm 2 / Vs, switch current ratio higher than 10 8 , NBIS and PBIS have good stability, and the threshold voltage change is less than 1 V per hour.

[0116] It can be seen that the double active layer terbium doped oxide thin film transistor has high electron mobility, large on-state current and low off-state current, and can achieve a high switching current ratio and a subthreshold swing of 0.3V / dec, indicating that the double active layer terbium doped oxide channel has good interface characteristics and low defect state density.

[0117] Embodiment 3

[0118] Embodiment 3 of the present invention provides a method for preparing a high-mobility and high-stability dual-active-layer terbium-doped oxide thin-film transistor, the method comprising:

[0119] Step S1: preparing a gate electrode 11 and a gate insulating layer 12 on the surface of a substrate 10 .

[0120] Wherein, step S1 specifically includes:

[0121] Step S11: depositing a metal film as the gate electrode 11 on the surface of the cleaned substrate 10 by vacuum physical vapor deposition, and patterning the metal film by photolithography.

[0122] Preferably, the metal film Al metal film is patterned by ultraviolet lithography and wet etching.

[0123] Step S12: depositing a gate insulating layer 12 and performing surface treatment using ultraviolet light or plasma.

[0124] Preferably, an oxide is formed as the insulating layer by anodization; the anodized substrate is ultrasonically cleaned in deionized water and isopropanol for 10 minutes respectively, dried in an oven at 70° C., and then irradiated under ultraviolet light for 30 minutes.

[0125] Step S3: preparing a first active layer 13 on a surface of the gate insulating layer 12 away from the substrate 10 , and preparing a second active layer 14 on the first active layer 13 .

[0126] Wherein, step S3 specifically includes:

[0127] Step S31: A 5 nm thick terbium-doped oxide film is deposited on the gate insulating layer 12 by magnetron sputtering as the first active layer 13, and annealed in an atmospheric environment. The target material used for sputtering is InZnTbO, wherein the cation molar ratio is In:Zn:Tb = 15:4:1.

[0128] Step S32: using ultraviolet light or plasma to perform surface treatment on the bottom channel layer.

[0129] Preferably, O-plasma is used to perform surface treatment on the first active layer 13 with a power of 100 W and a time of 60 seconds.

[0130] Step S33: A 10 nm terbium-doped oxide film is deposited on the first active layer 13 by magnetron sputtering as the second active layer 14, and annealed in an atmospheric environment. The target material used for sputtering is InZnTbO, wherein the cation molar ratio is In:Zn:Tb = 15:3:2. The dual active layer channel is patterned by ultraviolet lithography and wet etching.

[0131] Preferably, the annealing treatment is performed by photon sintering, laser annealing, microwave heating annealing, or ordinary thermal annealing, and the annealing temperature is 150°C to 500°C.

[0132] Step S4: Prepare source and drain electrodes to obtain a TFT device.

[0133] The transfer characteristic curve of the double active layer terbium-doped oxide thin film transistor in this embodiment is obtained through testing as follows: Figure 7 As shown in the figure, after testing and calculation, the carrier mobility of the double active layer terbium-doped oxide thin film transistor provided in the third embodiment of the present invention is as high as 58 cm 2 / Vs, switch current ratio higher than 10 8 , NBIS and PBIS have good stability, and the threshold voltage change is less than 1V per hour.

[0134] In summary, the present invention provides a high-mobility, high-stability dual-active-layer Tb-doped oxide thin-film transistor and a preparation method thereof. The dual-active-layer Tb-doped oxide thin-film transistor fully utilizes the characteristics of high oxygen binding energy and low charge transfer transition energy of terbium ions, and improves the electrical bias stability of the device by doping a small amount of terbium element.

[0135] The present invention uses two layers of terbium-doped oxide films with different terbium content and film thickness to stack layer by layer to construct a dual active layer channel, wherein the terbium-doped oxide film with low terbium content and low film thickness is used as the bottom channel layer, and the terbium-doped oxide film with high terbium content and high film thickness is used as the top channel layer. By accurately controlling the channel layer material composition and film thickness, the carrier mobility and stability of the oxide TFT are improved.

[0136] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a dual active layer oxide thin film transistor, characterized in that: The preparation method specifically comprises: Step S1: preparing a gate electrode and a gate insulating layer on the surface of a substrate; Step S2: preparing a precursor solution, wherein the precursor solution is prepared using terbium nitrate hydrate; The step S2 specifically includes: The ratio of In:Li:Tb ions in solution A of the precursor solution is 95:5:0; The precursor solution has a ratio of In:Li:Tb ions of 85:5:10 in solution B; Step S3: preparing a first active layer on a surface of the gate insulating layer away from the substrate, and preparing a second active layer on a surface of the first active layer; Step S3 specifically includes: Step S31: pre-growing the solution A on the surface of the gate insulating layer away from the substrate by spin coating, and then performing annealing treatment in an atmospheric environment to obtain a first active layer; Step S32: using oxygen plasma to perform surface treatment on the first active layer; Step S33: pre-growing the solution B on the first active layer by spin coating, and then performing annealing treatment in an atmospheric environment to obtain a second active layer; Step S4: preparing source and drain electrodes to obtain a double active layer oxide thin film transistor device; The terbium element exists in the form of a mixed valence state of trivalent ions and tetravalent ions; the thickness of the first active layer film is less than the thickness of the second active layer film; The step S2 can be placed in any step before use; The double active layer oxide thin film transistor device gives full play to the characteristics of high oxygen binding energy and low charge transfer transition energy of terbium ions, and improves the electrical bias stability of the device by doping a small amount of terbium elements.

2. The preparation method according to claim 1, characterized in that: Step S1 includes: preparing one or more conductive films by physical vapor deposition, and patterning them by hollow mask or photolithography to obtain a gate electrode; preparing a gate insulating layer by anodization, thermal oxidation, physical vapor deposition or chemical vapor deposition, and patterning them by hollow mask or photolithography.

3. The preparation method according to claim 1, characterized in that: Step S4 includes: preparing one or more layers of conductive film by vacuum evaporation or sputtering, and patterning by hollow mask or photolithography to obtain source and drain electrodes.

4. A double active layer terbium-doped oxide thin film transistor, characterized in that: The thin film transistor is prepared according to the preparation method according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Oxide thin-film transistor and preparation method, display device and camera device

    CN106298958A

  • Oxide semiconductor thin film and thin film transistor prepared from same

    CN107146816A

  • Oxide semiconductor thin film, and oxide thin-film transistor and preparation method thereof

    CN107527946A

  • Laminated silicon-doped tin oxide thin film transistor and preparation method thereof

    CN109887991A

  • Array substrate and display panel

    CN115295564A