A β-MnO2@δ-MnO2 heterostructure material and its preparation method and use
The size of δ-MnO2 is adjusted through the CTAB intercalation effect to achieve vertical growth of β-MnO2@δ-MnO2 heterostructure materials, which solves the growth problems caused by size differences and improves the structural stability and electrochemical performance of the material. It is suitable for for supercapacitors.
Patent Information
- Application Number
- CN202311529675.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-16
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-11-16
AI Technical Summary
The size difference between β-MnO2 and δ-MnO2 is too large, which makes traditional δ-MnO2 unable to grow smoothly on β-MnO2, limiting the structural stability and electrochemical performance of the material.
Through the intercalation effect of cetyltrimethylammonium bromide (CTAB) on layered materials, the size of δ-MnO2 is adjusted to achieve ultra-thin layered δ-MnO2 nanosheets on solid structure β-MnO2 nanorods. By vertical growth, a structurally stable β-MnO2@δ-MnO2 heterostructure material was prepared.
The material's structural stability and electrochemical properties were successfully improved, showing excellent cycle stability and rate performance, making it suitable for use as the working electrode of supercapacitors.
Smart Images

Figure CN117476372B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrochemical energy storage materials, and in particular to a β-MnO2@δ-MnO2 heterostructure material and a preparation method and application thereof. Background Art
[0002] Electrochemical energy storage materials are one of the main materials for preparing electrochemical energy storage devices such as secondary batteries, capacitors, fuel cells, and solid-state batteries. Their effective charge storage density, reversibility of chemical reactions and other properties are the key to achieving efficient energy storage and largely determine the quality of electrochemical energy storage devices. Currently, the commonly used electrochemical energy storage materials mainly include metal oxides, carbon-based materials, organic polymers, etc. These materials have their own advantages and disadvantages. For example, carbon-based materials have the advantages of large specific surface area and good chemical stability. However, due to their low specific capacity, their electrochemical performance is greatly limited; organic polymers are also restricted in their application in supercapacitor electrode materials due to their own structural constraints. Metal oxides have attracted widespread attention because they undergo reversible reactions at the electrode / solution interface and can produce large Faraday pseudocapacitance.
[0003] MnO2 is an ideal electrode material for supercapacitors because of its low price and environmental friendliness. The energy storage reaction of MnO2 includes two steps: first, MnO2 is reduced to manganese oxyhydroxide (MnOOH), and MnOOH is deposited on the surface of the lattice; second, MnOOH is transferred to the surface of MnO2, at which time MnOOH is reduced to Mn(OH)2, and Mn3O4 is formed and accumulated during the discharge and charge process, which not only consumes the electrode material, but also forms the internal resistance of the electrode, causing the discharge capacitance of the MnO2 electrode to decay rapidly. Through the study of MnO2, it was found that nano-sized MnO2 is a typical polycrystalline inorganic material. The traditional polycrystalline forms mainly include α-MnO2, β-MnO2, γ-MnO2, λ-MnO2, ε-MnO2, and δ-MnO2. They have octahedral units [MnO6] with different arrangements, and the interconnection methods between the octahedral units [MnO6] are also different, thus forming different channels or interlayers with gaps of different sizes.
[0004] β-MnO2 is a rutile tetragonal structure, and its octahedral units [MnO6] regularly form well-arranged channels, making it one of the most thermodynamically stable structures, and β-MnO2 has excellent conductivity and rate performance. However, the crystal structure of β-MnO2 is a diameter of The 1×1 narrow tunnel structure is not conducive to ion diffusion and electron transport, resulting in a specific capacitance value of only 9F·g -1, which is less used in the field of supercapacitors. δ-MnO2, due to its layered structure, theoretically can easily provide active sites for ion migration, resulting in a higher specific capacitance value. However, its layered structure is prone to structural collapse under high scanning speeds and long-term cycles, resulting in poor stability. Based on the above theory, the inventors of the present invention proposed to construct a composite material of β-MnO2 and δ-MnO2 to solve the problem of poor electrochemical properties of β-MnO2. However, the size difference between β-MnO2 and δ-MnO2 is too large, resulting in the inability of traditional δ-MnO2 to grow smoothly on β-MnO2. Summary of the invention
[0005] In order to solve the problem that the size difference between β-MnO2 and δ-MnO2 is too large, which leads to the inability of traditional δ-MnO2 to grow smoothly on β-MnO2, the purpose of the present invention is to provide a β-MnO2@δ-MnO2 heterostructure material and its preparation method and use. The present invention aims to control the size of δ-MnO2 by using the intercalation effect of hexadecyltrimethylammonium bromide (CTAB) on layered materials and the long chain structure of CTAB to promote the peeling and shedding of δ-MnO2 nanosheets, thereby realizing the vertical growth of ultra-thin layered δ-MnO2 nanosheets on solid β-MnO2 nanorods, and successfully preparing a β-MnO2@δ-MnO2 heterostructure material with stable structure.
[0006] To achieve the above objectives, the technical solution of the present invention is as follows.
[0007] The first aspect of the present invention provides a method for preparing a β-MnO2@δ-MnO2 heterostructure material, comprising the following steps:
[0008] Manganese sulfate and ammonium persulfate are dissolved in water, and then a hydrothermal reaction is carried out to obtain β-MnO2 nanomaterials; β-MnO2 nanomaterials, potassium permanganate, CTAB and water are evenly mixed, and then a secondary hydrothermal reaction is carried out to obtain β-MnO2@δ-MnO2 heterogeneous structure materials.
[0009] In a preferred embodiment, the mass ratio of manganese sulfate to ammonium persulfate is 0.8-0.85:1.1.
[0010] In a preferred embodiment, the mass ratio of β-MnO2 nanomaterial to potassium permanganate and CTAB is 0.1-0.6:0.55-0.6:0.04.
[0011] In a preferred embodiment, the temperature of the first hydrothermal reaction is 140-145° C.; the time of the first hydrothermal reaction is 10-16 h; the temperature of the second hydrothermal reaction is 140-145° C.; the time of the second hydrothermal reaction is 10-16 h.
[0012] In a preferred embodiment, the β-MnO2 nanomaterial is a nanorod structure material.
[0013] The second aspect of the present invention provides a β-MnO2@δ-MnO2 heterostructure material, which is prepared by the preparation method described in the first aspect.
[0014] The third aspect of the present invention provides a use of the β-MnO2@δ-MnO2 heterostructure material described in the second aspect, wherein the β-MnO2@δ-MnO2 heterostructure material is used as an active material for preparing a working electrode.
[0015] In a preferred embodiment, the working electrode is prepared by dispersing a binder, a conductive agent, and an active material in an organic solvent to obtain a slurry, and then coating the slurry on a current collector.
[0016] In a preferred embodiment, the binder is PVDF; the conductive agent is acetylene black; the organic solvent is NMP; the current collector is carbon paper; and the mass ratio of the binder, conductive agent, and active material is 0.005:0.005:0.04.
[0017] In a preferred embodiment, the β-MnO2@δ-MnO2 heterostructure material is used as an active material to prepare a working electrode of a supercapacitor.
[0018] Beneficial effects of the present invention:
[0019] 1. The present invention uses the intercalation effect of CTAB on layered materials and the long chain structure of CTAB to promote the exfoliation and shedding of δ-MnO2 nanosheets, thereby controlling the size of δ-MnO2 and achieving the vertical growth of ultra-thin layered δ-MnO2 nanosheets on solid β-MnO2 nanorods, and successfully prepares a structurally stable β-MnO2@δ-MnO2 heterostructure material.
[0020] 2. The present invention adopts a simple hydrothermal method to prepare the β-MnO2@δ-MnO2 heterostructure material, which can be used as a supercapacitor electrode material. It is precisely because its growth substrate is a stable solid structure β-MnO2 that it exhibits excellent cycle stability, rate performance and other properties under long-term cycle charge and discharge conditions. The method of use of the present invention is highly innovative, the manufacturing process is simple, green and safe, the experimental temperature is low, the product morphology is good and the purity is high, and it is suitable for industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the X-ray diffraction pattern of the β-MnO2@δ-MnO2 heterostructure material prepared in Example 1.
[0022] Figure 2 These are scanning electron micrographs of the β-MnO2@δ-MnO2 heterostructure material prepared in Example 1 at different magnifications.
[0023] Figure 3 This is a transmission electron micrograph of the β-MnO2@δ-MnO2 heterostructure material prepared in Example 1.
[0024] Figure 4 The cyclic voltammetry curves of the working electrode prepared in Example 1 at different scan rates.
[0025] Figure 5 It is the constant current charge and discharge curve of the working electrode prepared in Example 1 at different current densities.
[0026] Figure 6 1 is a capacitance retention curve of the working electrode prepared in Example 1 at different current densities.
[0027] Figure 7 This is the test result of the electrode prepared in Example 1 after 10,000 cycles.
[0028] Figure 8 In the figure, a is the cyclic voltammetry test curve of the working electrode prepared in Example 2; b is the cross-current charge-discharge curve.
[0029] Fig. 9 (a) is an electron microscope scanning image of the material prepared in Example 8; (b) is an electron microscope scanning image of the material prepared in Example 9; (c) is an electron microscope scanning image of the material prepared in Example 10.
[0030] Fig.10 (a) is a cyclic voltammetry test curve of the working electrode of Application Example 7; (b) is a constant current charge-discharge curve of the working electrode of Application Example 7; (c) is a cyclic voltammetry test curve of the working electrode of Application Example 8; (d) is a constant current charge-discharge curve of the working electrode of Application Example 8; (e) is a cyclic voltammetry test curve of the working electrode of Application Example 9; (f) is a constant current charge-discharge curve of the working electrode of Application Example 9. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0032] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.
[0033] β-MnO2 is a rutile tetragonal structure, and its octahedral units [MnO6] regularly form well-arranged channels, making it one of the most thermodynamically stable structures, and β-MnO2 has excellent conductivity and rate performance. However, the crystal structure of β-MnO2 is a diameter of The 1×1 narrow tunnel structure is not conducive to ion diffusion and electron transport, resulting in a specific capacitance value of only 9F·g -1 , which is less used in the field of supercapacitors. δ-MnO2, due to its layered structure, theoretically can easily provide active sites for ion migration, resulting in a higher specific capacitance value. However, its layered structure is prone to structural collapse under high scanning speeds and long-term cycles, resulting in poor stability. Based on the above theory, the inventors of the present invention proposed to construct a composite material of β-MnO2 and δ-MnO2 to solve the problem of poor electrochemical properties of β-MnO2. However, the size difference between β-MnO2 and δ-MnO2 is too large, resulting in the inability of traditional δ-MnO2 to grow smoothly on β-MnO2.
[0034] In order to solve the problem that the size difference between β-MnO2 and δ-MnO2 is too large, which leads to the inability of traditional δ-MnO2 to grow smoothly on β-MnO2, the present invention aims to use the intercalation effect of cetyltrimethylammonium bromide (CTAB) on layered materials and the long chain structure of CTAB to promote the exfoliation and shedding of δ-MnO2 nanosheets, thereby controlling the size of δ-MnO2, realizing the vertical growth of ultra-thin layered δ-MnO2 nanosheets on solid β-MnO2 nanorods, and successfully preparing a structurally stable β-MnO2@δ-MnO2 heterostructure material.
[0035] The first aspect of the present invention provides a method for preparing a β-MnO2@δ-MnO2 heterostructure material, comprising the following steps:
[0036] (1) A hydrothermal reaction: dissolving manganese sulfate and ammonium persulfate in water, and then performing a hydrothermal reaction to obtain β-MnO2 nanomaterials;
[0037] (2) Secondary hydrothermal reaction: β-MnO2 nanomaterials, potassium permanganate, CTAB and water are uniformly mixed, and then a secondary hydrothermal reaction is performed to obtain β-MnO2@δ-MnO2 heterostructure materials.
[0038] For the primary hydrothermal reaction of step (1): by adjusting the dosage ratio of manganese sulfate and ammonium persulfate, the hydrothermal reaction temperature and the hydrothermal reaction time, a β-MnO2 nanomaterial with a nanorod structure is prepared. In a preferred embodiment, the mass ratio of manganese sulfate to ammonium persulfate is 0.8 to 0.85:1.1. For example, 0.8:1.1, 0.83:1.1, 0.84:1.1, 0.845:1.1, 0.85:1.1, etc. In a preferred embodiment, the temperature of the primary hydrothermal reaction is 140 to 145°C; for example, 140°C, 145°C, etc. The time of the primary hydrothermal reaction is 10 to 16h; for example, 10h, 11h, 12h, 13h, 14h, 15h, 16h, etc.
[0039] In a preferred embodiment, the β-MnO2 nanomaterial is a nanorod structure material.
[0040] For the secondary hydrothermal reaction of step (2): by adjusting the dosage ratio of ammonium persulfate, potassium permanganate and CTAB, as well as the hydrothermal reaction temperature and hydrothermal reaction time, the size of δ-MnO2 can be adjusted due to the intercalation effect of CTAB, and an intercalation effect is formed to make δ-MnO2 thinner, and a layer of flower-like δ-MnO2 is uniformly grown on the surface of the nanorod-like β-MnO2. In a preferred embodiment, the mass ratio of β-MnO2 nanomaterial to potassium permanganate and CTAB is 0.1-0.6:0.55-0.6:0.04. For example, 0.1: 0.55: 0.04, 0.1: 0.56: 0.04, 0.1: 0.57: 0.04, 0.1: 0.58: 0.04, 0.1: 0.59: 0.04, 0.1: 0.6: 0.04, 0.2: 0.59: 0.04, 0.3: 0.59: 0.04, 0.4: 0.59: 0.04, 0.5: 0.59: 0.04, 0.6: 0.59: 0.04, etc. The temperature of the secondary hydrothermal reaction is 140-145°C; for example, 140°C, 145°C, etc. The time of the secondary hydrothermal reaction is 10-16h; for example, 10h, 11h, 12h, 13h, 14h, 15h, 16h, etc.
[0041] The second aspect of the present invention provides a β-MnO2@δ-MnO2 heterostructure material, which is prepared by the preparation method described in the first aspect.
[0042] The third aspect of the present invention provides a use of the β-MnO2@δ-MnO2 heterostructure material described in the second aspect, wherein the β-MnO2@δ-MnO2 heterostructure material is used as an active material for preparing a working electrode.
[0043] In a preferred embodiment, the working electrode is prepared by dispersing a binder, a conductive agent, and an active material in an organic solvent to obtain a slurry, and then coating the slurry on a current collector.
[0044] In a preferred embodiment, the binder is PVDF; the conductive agent is acetylene black; the organic solvent is NMP; the current collector is carbon paper; and the mass ratio of the binder, conductive agent, and active material is 0.005:0.005:0.04.
[0045] In a preferred embodiment, the β-MnO2@δ-MnO2 heterostructure material is used as an active material to prepare a working electrode of a supercapacitor.
[0046] In a preferred embodiment, the supercapacitor includes a reference electrode, a counter electrode, a working electrode and an electrolyte to form a three-electrode test system; the reference electrode is Ag / Ag + The electrode is a platinum electrode, the working electrode is the working electrode described in the fourth aspect; and the electrolyte is a 1M sodium sulfate solution. Specific embodiments
[0048] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0049] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0050] In the following examples, H8N2O8S2 is ammonium persulfate; MnSO4 is manganese sulfate;
[0051] Unless otherwise specified, the methods described in the following examples are all conventional methods; the reagents and materials described are all commercially available unless otherwise specified.
[0052] Example 1
[0053] A method for preparing a β-MnO2@δ-MnO2 heterostructure material comprises the following steps:
[0054] (1) Weigh 1.12 g of H8N2O8S2 and 0.845 g of MnSO4, add them into a beaker containing 30 mL of deionized water, and stir them magnetically to fully dissolve them to obtain a reaction solution;
[0055] The reaction solution was transferred into a 50 mL polytetrafluoroethylene-lined high-pressure reactor and heated at a constant temperature in an oven at 140°C for 12 h. After the reaction was completed, it was cooled to room temperature. A black solid precipitate was obtained by filtration. The precipitate was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for drying to obtain a solid powder, i.e., β-MnO2 nanorod material.
[0056] (2) Weigh 0.4g of β-MnO2 nanorod material, 0.59g of KMnO4 and 0.04g of CTAB, and then add them into a 50mL polytetrafluoroethylene-lined autoclave filled with 30mL of deionized water, stir until the upper liquid has no suspended matter, and then heat it in an oven at 140°C for 12h. After the reaction is completed, cool it to room temperature. Filter to obtain a black solid precipitate, wash it with deionized water and anhydrous ethanol three times each, and then place it in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2@δ-MnO2 heterostructure material.
[0057] Example 2
[0058] A method for preparing a β-MnO2@δ-MnO2 heterostructure material comprises the following steps:
[0059] (1) Weigh 1.12 g of H8N2O8S2 and 0.845 g of MnSO4, add them into a beaker containing 30 mL of deionized water, and stir them magnetically to fully dissolve them to obtain a reaction solution;
[0060] The reaction solution was transferred into a 50 mL polytetrafluoroethylene-lined autoclave and heated at a constant temperature in an oven at 140°C for 12 h. After the reaction was completed, it was cooled to room temperature. A black solid precipitate was obtained by filtration. The precipitate was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for drying to obtain a solid powder, i.e., β-MnO2 nanorod material.
[0061] (2) Weigh 0.1g of β-MnO2 nanorod material, 0.59g of KMnO4 and 0.04g of CTAB, and then add them into a 50mL polytetrafluoroethylene-lined autoclave filled with 30mL of deionized water, stir until the upper liquid has no suspended matter, and heat it in an oven at 140°C for 12h. After the reaction is completed, cool it to room temperature. Filter to obtain a black solid precipitate, wash it with deionized water and anhydrous ethanol three times each, and then place it in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2@δ-MnO2 heterostructure material.
[0062] Example 3
[0063] A method for preparing a β-MnO2@δ-MnO2 heterostructure material comprises the following steps:
[0064] (1) Weigh 1.12 g of H8N2O8S2 and 0.845 g of MnSO4, add them into a beaker containing 30 mL of deionized water, and stir them magnetically to fully dissolve them to obtain a reaction solution;
[0065] The reaction solution was poured into a 50 mL polytetrafluoroethylene-lined autoclave, and heated at a constant temperature of 140°C in an oven for 12 hours. After the reaction was completed, it was cooled to room temperature. The black solid precipitate was filtered to obtain a black solid precipitate, which was washed with deionized water and anhydrous ethanol for 3 times each, and then placed in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2 nanorod material.
[0066] (2) Weigh 0.2g of β-MnO2 nanorod material, 0.59g of KMnO4 and 0.04g of CTAB, and then add them into a 50mL polytetrafluoroethylene-lined autoclave filled with 30mL of deionized water. Stir the upper layer liquid without suspended matter and heat it in an oven at 140℃ for 12h. After the reaction is completed, cool it to room temperature. Filter to obtain a black solid precipitate, wash it with deionized water and anhydrous ethanol three times each, and then place it in a vacuum drying oven at 60℃ for drying to obtain a solid powder, namely, β-MnO2@δ-MnO2 heterostructure material.
[0067] Example 4
[0068] A method for preparing a β-MnO2@δ-MnO2 heterostructure material comprises the following steps:
[0069] (1) Weigh 1.12 g of H8N2O8S2 and 0.845 g of MnSO4, add them into a beaker containing 30 mL of deionized water, and stir them magnetically to fully dissolve them to obtain a reaction solution;
[0070] The reaction solution was poured into a 50 mL polytetrafluoroethylene-lined autoclave, and heated at a constant temperature of 140°C in an oven for 12 hours. After the reaction was completed, it was cooled to room temperature. The black solid precipitate was filtered to obtain a black solid precipitate, which was washed with deionized water and anhydrous ethanol for 3 times each, and then placed in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2 nanorod material.
[0071] (2) Weigh 0.3g of β-MnO2 nanorod material, 0.59g of KMnO4 and 0.04g of CTAB, and then add them into a 50mL polytetrafluoroethylene-lined autoclave filled with 30mL of deionized water. Stir the upper layer liquid without suspended matter and heat it in an oven at 140℃ for 12h. After the reaction is completed, cool it to room temperature. Filter to obtain a black solid precipitate, wash it with deionized water and anhydrous ethanol three times each, and then place it in a vacuum drying oven at 60℃ for drying to obtain a solid powder, namely, β-MnO2@δ-MnO2 heterostructure material.
[0072] Example 5
[0073] A method for preparing a β-MnO2@δ-MnO2 heterostructure material comprises the following steps:
[0074] (1) Weigh 1.12 g of H8N2O8S2 and 0.845 g of MnSO4, add them into a beaker containing 30 mL of deionized water, and stir them magnetically to fully dissolve them to obtain a reaction solution;
[0075] The reaction solution was poured into a 50 mL polytetrafluoroethylene-lined autoclave, and heated at a constant temperature of 140°C in an oven for 12 hours. After the reaction was completed, it was cooled to room temperature. The black solid precipitate was filtered to obtain a black solid precipitate, which was washed with deionized water and anhydrous ethanol for 3 times each, and then placed in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2 nanorod material.
[0076] (2) Weigh 0.5g of β-MnO2 nanorod material, 0.59g of KMnO4 and 0.04g of CTAB and add them to a 50mL polytetrafluoroethylene-lined autoclave filled with 30mL of deionized water. Stir the upper liquid to remove suspended matter and heat it in an oven at 140°C for 12h. After the reaction is completed, cool it to room temperature. Filter to obtain a black solid precipitate, wash it with deionized water and anhydrous ethanol three times each, and then place it in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2@δ-MnO2 heterostructure material.
[0077] Example 6
[0078] A method for preparing a β-MnO2@δ-MnO2 heterostructure material comprises the following steps:
[0079] (1) Weigh 1.12 g of H8N2O8S2 and 0.845 g of MnSO4, add them into a beaker containing 30 mL of deionized water, stir them magnetically to fully dissolve them, and obtain a reaction solution;
[0080] The reaction solution was poured into a 50 mL polytetrafluoroethylene-lined autoclave, and heated at a constant temperature of 140°C in an oven for 12 hours. After the reaction was completed, it was cooled to room temperature. The black solid precipitate was filtered to obtain a black solid precipitate, which was washed with deionized water and anhydrous ethanol for 3 times each, and then placed in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2 nanorod material.
[0081] (2) Weigh 0.6g of β-MnO2 nanorod material, 0.59g of KMnO4 and 0.04g of CTAB, and then add them into a 50mL polytetrafluoroethylene-lined autoclave filled with 30mL of deionized water. Stir the upper liquid without suspended matter and heat it in an oven at 140°C for 12h. After the reaction is completed, cool it to room temperature. Filter to obtain a black solid precipitate, wash it with deionized water and anhydrous ethanol three times each, and then place it in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2@δ-MnO2 heterostructure material.
[0082] Example 7
[0083] A method for preparing a β-MnO2@δ-MnO2 heterostructure material comprises the following steps:
[0084] (1) Weigh 1.12 g of H8N2O8S2 and 0.845 g of MnSO4, add them into a beaker containing 30 mL of deionized water, and stir them magnetically to fully dissolve them to obtain a reaction solution;
[0085] The reaction solution was transferred into a 50 mL polytetrafluoroethylene-lined high-pressure reactor and heated at a constant temperature of 145°C in an oven for 12 h. After the reaction was completed, it was cooled to room temperature. A black solid precipitate was obtained by filtration. The precipitate was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for drying to obtain a solid powder, i.e., β-MnO2 nanorod material.
[0086] (2) Weigh 0.4g of β-MnO2 nanorod material, 0.59g of KMnO4 and 0.04g of CTAB, and then add them into a 50mL polytetrafluoroethylene-lined autoclave filled with 30mL of deionized water, stir until the upper liquid has no suspended matter, and then heat it in an oven at 145°C for 12h. After the reaction is completed, cool it to room temperature. Filter to obtain a black solid precipitate, wash it with deionized water and anhydrous ethanol three times each, and then place it in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2@δ-MnO2 heterostructure material.
[0087] Example 8
[0088] A method for preparing a β-MnO2@δ-MnO2 heterostructure material comprises the following steps:
[0089] (1) Weigh 1.12 g of H8N2O8S2 and 0.845 g of MnSO4, add them into a beaker containing 30 mL of deionized water, and stir them magnetically to fully dissolve them to obtain a reaction solution;
[0090] The reaction solution was transferred into a 50 mL polytetrafluoroethylene-lined high-pressure reactor and heated at a constant temperature in an oven at 140°C for 16 h. After the reaction was completed, it was cooled to room temperature. A black solid precipitate was obtained by filtration. The precipitate was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for drying to obtain a solid powder, i.e., β-MnO2 nanorod material.
[0091] (2) Weigh 0.4g of β-MnO2 nanorod material, 0.59g of KMnO4 and 0.04g of CTAB, and then add them into a 50mL polytetrafluoroethylene-lined autoclave filled with 30mL of deionized water, stir until the upper liquid has no suspended matter, and then heat it in an oven at 140°C for 16h. After the reaction is completed, cool it to room temperature. Filter to obtain a black solid precipitate, wash it with deionized water and anhydrous ethanol three times each, and then place it in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2@δ-MnO2 heterostructure material.
[0092] Example 9
[0093] A method for preparing a β-MnO2@δ-MnO2 heterostructure material comprises the following steps:
[0094] (1) Weigh 1.12 g of H8N2O8S2 and 0.845 g of MnSO4, add them into a beaker containing 30 mL of deionized water, and stir them magnetically to fully dissolve them to obtain a reaction solution;
[0095] The reaction solution was transferred into a 50 mL polytetrafluoroethylene-lined high-pressure reactor and heated at a constant temperature of 140°C in an oven for 20 h. After the reaction was completed, it was cooled to room temperature. A black solid precipitate was obtained by filtration. The precipitate was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for drying to obtain a solid powder, i.e., β-MnO2 nanorod material.
[0096] (2) Weigh 0.4g of β-MnO2 nanorod material, 0.59g of KMnO4 and 0.04g of CTAB, and then add them into a 50mL polytetrafluoroethylene-lined autoclave filled with 30mL of deionized water, stir until the upper liquid has no suspended matter, and then heat it in an oven at 140°C for 20h. After the reaction is completed, cool it to room temperature. Filter to obtain a black solid precipitate, wash it with deionized water and anhydrous ethanol three times each, and then place it in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2@δ-MnO2 heterostructure material.
[0097] Example 10
[0098] A method for preparing a β-MnO2@δ-MnO2 heterostructure material comprises the following steps:
[0099] (1) Weigh 1.12 g of H8N2O8S2 and 0.845 g of MnSO4, add them into a beaker containing 30 mL of deionized water, and stir them magnetically to fully dissolve them to obtain a reaction solution;
[0100] The reaction solution was transferred into a 50 mL polytetrafluoroethylene-lined high-pressure reactor and heated at a constant temperature of 140°C in an oven for 24 h. After the reaction was completed, it was cooled to room temperature. A black solid precipitate was obtained by filtration. The precipitate was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for drying to obtain a solid powder, i.e., β-MnO2 nanorod material.
[0101] (2) Weigh 0.4g of β-MnO2 nanorod material, 0.59g of KMnO4 and 0.04g of CTAB, and then add them into a 50mL polytetrafluoroethylene-lined autoclave filled with 30mL of deionized water, stir until the upper liquid has no suspended matter, and then heat it in an oven at 140°C for 24h. After the reaction is completed, cool it to room temperature. Filter to obtain a black solid precipitate, wash it with deionized water and anhydrous ethanol three times each, and then place it in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2@δ-MnO2 heterostructure material.
[0102] Embodiment 11
[0103] A method for preparing a β-MnO2@δ-MnO2 heterostructure material comprises the following steps:
[0104] (1) Weigh 1.12 g of H8N2O8S2 and 0.8 g of MnSO4, add them into a beaker containing 30 mL of deionized water, and stir them magnetically to fully dissolve them to obtain a reaction solution;
[0105] The reaction solution was transferred into a 50 mL polytetrafluoroethylene-lined high-pressure reactor and heated at a constant temperature in an oven at 140°C for 12 h. After the reaction was completed, it was cooled to room temperature. A black solid precipitate was obtained by filtration. The precipitate was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for drying to obtain a solid powder, i.e., β-MnO2 nanorod material.
[0106] (2) Weigh 0.4g of β-MnO2 nanorod material, 0.55g of KMnO4 and 0.04g of CTAB, and then add them into a 50mL polytetrafluoroethylene-lined autoclave filled with 30mL of deionized water, stir until the upper liquid has no suspended matter, and then heat it in an oven at 140°C for 12h. After the reaction is completed, cool it to room temperature. Filter to obtain a black solid precipitate, wash it with deionized water and anhydrous ethanol three times each, and then place it in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2@δ-MnO2 heterostructure material.
[0107] Comparative Example 1
[0108] A method for preparing a β-MnO2 nanomaterial, which differs from Example 1 in that no δ-MnO2 material is added, and the specific method comprises the following steps:
[0109] (1) Weigh 1.12 g of H8N2O8S2 and 0.845 g of MnSO4, add them into a beaker containing 30 mL of deionized water, and stir them magnetically to fully dissolve them to obtain a reaction solution;
[0110] The reaction solution was transferred into a 50 mL polytetrafluoroethylene-lined high-pressure reactor and heated at a constant temperature in an oven at 140°C for 12 h. After the reaction was completed, it was cooled to room temperature. A black solid precipitate was obtained by filtration. The precipitate was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for drying to obtain a solid powder, i.e., β-MnO2 nanorod material.
[0111] (2) Weigh 0.4 g of β-MnO2 nanorod material, then add it into a 50 mL polytetrafluoroethylene-lined autoclave filled with 30 mL of deionized water, stir until the upper liquid has no suspended matter, then heat it in an oven at 140°C for 12 h, and after the reaction is completed, cool it to room temperature. Filter it to obtain a black solid precipitate, wash it with deionized water and anhydrous ethanol three times each, and then place it in a vacuum drying oven at 60°C for drying to obtain a solid powder, i.e., β-MnO2 nanomaterial.
[0112] Comparative Example 2
[0113] A method for preparing a β-MnO2@δ-MnO2 composite material, which differs from Example 1 in that CTAB is not added, and the specific method comprises the following steps:
[0114] (1) Weigh 1.12 g of H8N2O8S2 and 0.845 g of MnSO4, add them into a beaker containing 30 mL of deionized water, and stir them magnetically to fully dissolve them to obtain a reaction solution;
[0115] The reaction solution was transferred into a 50 mL polytetrafluoroethylene-lined high-pressure reactor and heated at a constant temperature in an oven at 140°C for 12 h. After the reaction was completed, it was cooled to room temperature. A black solid precipitate was obtained by filtration. The precipitate was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for drying to obtain a solid powder, i.e., β-MnO2 nanorod material.
[0116] (2) Weigh 0.4g of β-MnO2 nanorod material, 0.59g of KMnO4 and 0.14g of MnSO4, and then add them into a 50mL polytetrafluoroethylene-lined autoclave filled with 30mL of deionized water, stir until the upper liquid has no suspended matter, and then heat it in an oven at 140°C for 12h. After the reaction is completed, cool it to room temperature. Filter to obtain a black solid precipitate, wash it with deionized water and anhydrous ethanol three times each, and then place it in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2@δ-MnO2 composite material.
[0117] Comparative Example 3
[0118] A method for preparing a β-MnO2@δ-MnO2 composite material comprises the following steps:
[0119] (1) Weigh 1.12 g of H8N2O8S2 and 0.845 g of MnSO4, add them into a beaker containing 30 mL of deionized water, and stir them magnetically to fully dissolve them to obtain a reaction solution;
[0120] The reaction solution was transferred into a 50 mL polytetrafluoroethylene-lined high-pressure reactor and heated at a constant temperature in an oven at 160°C for 12 h. After the reaction was completed, it was cooled to room temperature. A black solid precipitate was obtained by filtration. The precipitate was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for drying to obtain a solid powder, i.e., β-MnO2 nanorod material.
[0121] (2) Weigh 0.4g of β-MnO2 nanorod material, 0.59g of KMnO4 and 0.04g of CTAB, and then add them into a 50mL polytetrafluoroethylene-lined autoclave filled with 30mL of deionized water, stir until the upper liquid has no suspended matter, and then heat it in an oven at 160°C for 12h. After the reaction is completed, cool it to room temperature. Filter to obtain a black solid precipitate, wash it with deionized water and anhydrous ethanol three times each, and then place it in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2@δ-MnO2 composite material.
[0122] Comparative Example 4
[0123] A method for preparing a β-MnO2@δ-MnO2 composite material comprises the following steps:
[0124] (1) Weigh 1.12 g of H8N2O8S2 and 0.845 g of MnSO4, add them into a beaker containing 30 mL of deionized water, and stir them magnetically to fully dissolve them to obtain a reaction solution;
[0125] The reaction solution was transferred into a 50 mL polytetrafluoroethylene-lined high-pressure reactor and heated at a constant temperature in an oven at 120°C for 12 h. After the reaction was completed, it was cooled to room temperature. A black solid precipitate was obtained by filtration. The precipitate was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for drying to obtain a solid powder, i.e., β-MnO2 nanorod material.
[0126] (2) Weigh 0.4g of β-MnO2 nanorod material, 0.59g of KMnO4 and 0.04g of CTAB, and then add them into a 50mL polytetrafluoroethylene-lined autoclave filled with 30mL of deionized water, stir until the upper liquid has no suspended matter, and then heat it in an oven at 120°C for 12h. After the reaction is completed, cool it to room temperature. Filter to obtain a black solid precipitate, wash it with deionized water and anhydrous ethanol three times each, and then place it in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2@δ-MnO2 composite material.
[0127] Comparative Example 5
[0128] A method for preparing a β-MnO2@δ-MnO2 composite material comprises the following steps:
[0129] (1) Weigh 1.12 g of H8N2O8S2 and 0.845 g of MnSO4, add them into a beaker containing 30 mL of deionized water, and stir them magnetically to fully dissolve them to obtain a reaction solution;
[0130] The reaction solution was transferred into a 50 mL polytetrafluoroethylene-lined high-pressure reactor and heated at a constant temperature in an oven at 140°C for 12 h. After the reaction was completed, it was cooled to room temperature. A black solid precipitate was obtained by filtration. The precipitate was washed three times with deionized water and anhydrous ethanol respectively, and then placed in a vacuum drying oven at 60°C for drying to obtain a solid powder, i.e., β-MnO2 nanorod material.
[0131] (2) Weigh 0.4g of β-MnO2 nanorod material, 0.7g of KMnO4 and 0.05g of CTAB, and then add them into a 50mL polytetrafluoroethylene-lined autoclave filled with 30mL of deionized water, stir until the upper liquid has no suspended matter, and then heat it in an oven at 140°C for 12h. After the reaction is completed, cool it to room temperature. Filter to obtain a black solid precipitate, wash it with deionized water and anhydrous ethanol three times each, and then place it in a vacuum drying oven at 60°C for drying to obtain a solid powder, namely, β-MnO2@δ-MnO2 composite material.
[0132] Application Example 1
[0133] A method for preparing a working electrode comprises the following steps:
[0134] Weigh 0.005 g of PVDF, 0.005 g of acetylene black and 0.04 g of active material, where the active material is the β-MnO2@δ-MnO2 heterostructure material of Example 1.
[0135] The weighed PVDF, acetylene black and active material were placed in an agate mortar in sequence, 0.6 ml of NMP solution was added, and the mixture was ground for 5-7 min to obtain a slurry;
[0136] The slurry was evenly coated on the carbon paper with a coating area of 1 cm×1 cm. The carbon paper coated with the slurry was placed in a vacuum drying oven and dried at 60° C. to obtain a working electrode.
[0137] A supercapacitor comprises a reference electrode, a counter electrode, a working electrode and an electrolyte to form a three-electrode test system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, the working electrode is the working electrode prepared by the above method; and the electrolyte is a 1M sodium sulfate solution.
[0138] Application Example 2
[0139] A method for preparing a working electrode comprises the following steps:
[0140] Weigh 0.005 g of PVDF, 0.005 g of acetylene black and 0.04 g of active material, where the active material is the β-MnO2@δ-MnO2 heterostructure material of Example 2.
[0141] The weighed PVDF, acetylene black and active material were placed in an agate mortar in sequence, 0.6 ml of NMP solution was added, and the mixture was ground for 5-7 min to obtain a slurry;
[0142] The slurry was evenly coated on the carbon paper with a coating area of 1 cm×1 cm. The carbon paper coated with the slurry was placed in a vacuum drying oven and dried at 60° C. to obtain a working electrode.
[0143] A supercapacitor comprises a reference electrode, a counter electrode, a working electrode and an electrolyte to form a three-electrode test system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, the working electrode is the working electrode prepared by the above method; and the electrolyte is a 1M sodium sulfate solution.
[0144] Application Example 3
[0145] A method for preparing a working electrode comprises the following steps:
[0146] Weigh 0.005 g of PVDF, 0.005 g of acetylene black and 0.04 g of active material, where the active material is the β-MnO2@δ-MnO2 heterostructure material of Example 3.
[0147] The weighed PVDF, acetylene black and β-MnO2@δ-MnO2 heterostructure material were placed in an agate mortar in sequence, 0.6 ml of NMP solution was added, and the mixture was ground for 5-7 min to obtain a slurry;
[0148] The slurry was evenly coated on the carbon paper with a coating area of 1 cm×1 cm. The carbon paper coated with the slurry was placed in a vacuum drying oven and dried at 60° C. to obtain a working electrode.
[0149] A supercapacitor comprises a reference electrode, a counter electrode, a working electrode and an electrolyte to form a three-electrode test system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, the working electrode is the working electrode prepared by the above method; and the electrolyte is a 1M sodium sulfate solution.
[0150] Application Example 4
[0151] A method for preparing a working electrode comprises the following steps:
[0152] Weigh 0.005 g of PVDF, 0.005 g of acetylene black and 0.04 g of active material, where the active material is the β-MnO2@δ-MnO2 heterostructure material of Example 4.
[0153] The weighed PVDF, acetylene black and active material were placed in an agate mortar in sequence, 0.6 ml of NMP solution was added, and the mixture was ground for 5-7 min to obtain a slurry;
[0154] The slurry was evenly coated on the carbon paper with a coating area of 1 cm×1 cm. The carbon paper coated with the slurry was placed in a vacuum drying oven and dried at 60° C. to obtain a working electrode.
[0155] A supercapacitor comprises a reference electrode, a counter electrode, a working electrode and an electrolyte to form a three-electrode test system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, the working electrode is the working electrode prepared by the above method; and the electrolyte is a 1M sodium sulfate solution.
[0156] Application Example 5
[0157] A method for preparing a working electrode comprises the following steps:
[0158] Weigh 0.005 g of PVDF, 0.005 g of acetylene black and 0.04 g of active material, where the active material is the β-MnO2@δ-MnO2 heterostructure material of Example 5.
[0159] The weighed PVDF, acetylene black and active material were placed in an agate mortar in sequence, 0.6 ml of NMP solution was added, and the mixture was ground for 5-7 min to obtain a slurry;
[0160] The slurry was evenly coated on the carbon paper with a coating area of 1 cm×1 cm. The carbon paper coated with the slurry was placed in a vacuum drying oven and dried at 60° C. to obtain a working electrode.
[0161] A supercapacitor comprises a reference electrode, a counter electrode, a working electrode and an electrolyte to form a three-electrode test system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, the working electrode is the working electrode prepared by the above method; and the electrolyte is a 1M sodium sulfate solution.
[0162] Application Example 6
[0163] A method for preparing a working electrode comprises the following steps:
[0164] 0.005 g of PVDF, 0.005 g of acetylene black and 0.04 g of active material were weighed, where the active material was the β-MnO2@δ-MnO2 heterostructure material of Example 6.
[0165] The weighed PVDF, acetylene black and active material were placed in an agate mortar in sequence, 0.6 ml of NMP solution was added, and the mixture was ground for 5-7 min to obtain a slurry;
[0166] The slurry was evenly coated on the carbon paper with a coating area of 1 cm×1 cm. The carbon paper coated with the slurry was placed in a vacuum drying oven and dried at 60° C. to obtain a working electrode.
[0167] A supercapacitor comprises a reference electrode, a counter electrode, a working electrode and an electrolyte to form a three-electrode test system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, the working electrode is the working electrode prepared by the above method; and the electrolyte is a 1M sodium sulfate solution.
[0168] Application Example 7
[0169] A method for preparing a working electrode is basically the same as the method of Application Example 1, except that the active material is the β-MnO2@δ-MnO2 heterostructure material of Example 8.
[0170] A supercapacitor comprises a reference electrode, a counter electrode, a working electrode and an electrolyte to form a three-electrode test system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, the working electrode is the working electrode prepared by the above method; and the electrolyte is a 1M sodium sulfate solution.
[0171] Application Example 8
[0172] A method for preparing a working electrode is substantially the same as the method of Application Example 1, except that the active material is the β-MnO2@δ-MnO2 heterostructure material of Example 9.
[0173] A supercapacitor comprises a reference electrode, a counter electrode, a working electrode and an electrolyte to form a three-electrode test system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, the working electrode is the working electrode prepared by the above method; and the electrolyte is a 1M sodium sulfate solution.
[0174] Application Example 9
[0175] A method for preparing a working electrode is basically the same as the method of Application Example 1, except that the active material is the β-MnO2@δ-MnO2 heterostructure material of Example 10.
[0176] A supercapacitor comprises a reference electrode, a counter electrode, a working electrode and an electrolyte to form a three-electrode test system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, the working electrode is the working electrode prepared by the above method; and the electrolyte is a 1M sodium sulfate solution.
[0177] Application Comparative Example 1
[0178] A method for preparing a working electrode comprises the following steps:
[0179] Weigh 0.005g PVDF, 0.005g acetylene black and 0.04g active material, the active material is the β-MnO2 nanomaterial of Comparative Example 1. Put the weighed PVDF, acetylene black and active material into an agate mortar in turn, add 0.6ml NMP solution, grind for 5-7min to obtain slurry; evenly coat the slurry on carbon paper with a coating area of 1cm×1cm, put the carbon paper coated with the slurry into a vacuum drying oven and dry at 60°C to obtain a working electrode.
[0180] A supercapacitor comprises a reference electrode, a counter electrode, a working electrode and an electrolyte to form a three-electrode test system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, the working electrode is the working electrode prepared by the above method; and the electrolyte is a 1M sodium sulfate solution.
[0181] Application Comparative Example 2
[0182] A method for preparing a working electrode comprises the following steps:
[0183] Weigh 0.005g PVDF, 0.005g acetylene black and 0.04g active material, the active material is the β-MnO2@δ-MnO2 composite material of Comparative Example 2. Put the weighed PVDF, acetylene black and active material into an agate mortar in turn, add 0.6ml NMP solution, grind for 5-7min to obtain slurry; evenly coat the slurry on carbon paper with a coating area of 1cm×1cm, put the carbon paper coated with the slurry into a vacuum drying oven and dry at 60°C to obtain a working electrode.
[0184] A supercapacitor comprises a reference electrode, a counter electrode, a working electrode and an electrolyte to form a three-electrode test system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, the working electrode is the working electrode prepared by the above method; and the electrolyte is a 1M sodium sulfate solution.
[0185] Application Comparative Example 3
[0186] A method for preparing a working electrode comprises the following steps:
[0187] Weigh 0.005g PVDF, 0.005g acetylene black and 0.04g active material, the active material is the β-MnO2@δ-MnO2 composite material of Comparative Example 5. Put the weighed PVDF, acetylene black and active material into an agate mortar in turn, add 0.6ml NMP solution, grind for 5-7min to obtain slurry; evenly coat the slurry on carbon paper with a coating area of 1cm×1cm, put the carbon paper coated with the slurry into a vacuum drying oven and dry at 60°C to obtain a working electrode.
[0188] A supercapacitor comprises a reference electrode, a counter electrode, a working electrode and an electrolyte to form a three-electrode test system; the reference electrode is an Ag / AgCl electrode, the counter electrode is a platinum sheet electrode, the working electrode is the working electrode prepared by the above method; and the electrolyte is a 1M sodium sulfate solution.
[0189] The performance of the products prepared in the above examples was analyzed.
[0190] Test 1: X-ray diffraction analysis
[0191] The β-MnO2@δ-MnO2 heterostructure material prepared in Example 1 was subjected to X-ray diffraction (XRD) analysis, and the results are shown in Figure 1 . Figure 1 This is the X-ray diffraction pattern of the β-MnO2@δ-MnO2 heterostructure material prepared in Example 1.
[0192] Depend on Figure 1 It can be seen from the XRD spectrum that there are mainly eight peaks, including the characteristic peaks of β-MnO2 (110), (101), (111), (210), (211), (112) and the two characteristic peaks of δ-MnO2 (001) and (002), which confirms that the material is a composite of β-MnO2 and δ-MnO2.
[0193] Test 2: Scanning Electron Microscope Analysis
[0194] The β-MnO2@δ-MnO2 heterostructure material prepared in Example 1 was subjected to scanning electron microscopy (SEM) analysis, and the results are shown in Figure 2 . Figure 2 These are scanning electron microscope photographs of the β-MnO2@δ-MnO2 heterostructure material prepared in Example 1 at different magnifications.
[0195] Depend on Figure 2The SEM images show that nanosheet-like δ-MnO2 is uniformly grown on the nanorod-like β-MnO2, and ultrathin layered δ-MnO2 nanosheets grow vertically on the solid β-MnO2 nanorods, forming a structurally stable β-MnO2@δ-MnO2 heterostructure material.
[0196] Test 3: Transmission electron microscopy analysis
[0197] The β-MnO2@δ-MnO2 heterostructure material prepared in Example 1 was analyzed by transmission electron microscopy (TEM). Figure 3 . Figure 3 This is a transmission electron micrograph of the β-MnO2@δ-MnO2 heterostructure material prepared in Example 1.
[0198] Depend on Figure 3 The TEM images show that nanosheet-like δ-MnO2 is uniformly grown on the nanorod-like β-MnO2, and ultrathin layered δ-MnO2 nanosheets grow vertically on the solid structure of β-MnO2 nanorods, which further verifies the SEM image results.
[0199] Test 4: Electrochemical test analysis using the working electrode of Example 1
[0200] The β-MnO2@δ-MnO2 heterostructure material prepared in Example 1 was used to prepare a working electrode and electrochemical test analysis was performed. The results are shown in Figure 4-7 . Figure 4 The cyclic voltammetry curves of the working electrode prepared in Example 1 at different scan rates. Figure 5 It is the constant current charge and discharge curve of the working electrode prepared by using Example 1 at different current densities. Figure 6 1 is a capacitance retention curve of the working electrode prepared in Example 1 at different current densities. Figure 7 This is the test result of the working electrode prepared in Example 1 after 10,000 cycles.
[0201] Figure 4 What is shown is the cyclic voltammetry curve of the working electrode prepared by using Example 1 at a scanning rate of 10-200mV / s, showing a rectangular shape, a voltage window of 0-1V, and the material prepared by Example 1 is a capacitive positive electrode material.
[0202] Figure 5 The charge-discharge curve of the working electrode prepared in Example 1 at a current density of 1-10 A / g is shown. The curve is triangular, which further indicates the capacitive behavior of the β-MnO2@δ-MnO2 heterostructure material. Figure 5The test results are calculated Figure 6 The capacitance retention of the electrode material shown at different current densities. Figure 6 The results show that when the current density is expanded to 20 times, the capacitance value can still be maintained at 74.2% of the original capacitance value.
[0203] The working electrode prepared in Example 1 was subjected to a 10,000-cycle test. Figure 7 The cycle test results show that even after the working electrode of Example 1 has undergone 10,000 charge and discharge tests, its specific capacitance value can still maintain 97% of the initial capacitance value, showing excellent cycle stability.
[0204] Test 5: Electrochemical test analysis of the working electrode prepared in Example 2
[0205] Figure 8 a is the cyclic voltammetry (CV) test curve of the working electrode prepared in Example 2; b is the cross-current charge-discharge (GCD) curve. Figure 8 The test results show that the CV curve shows polarization, and the GCD curve has an obvious flat process when charging close to 1V. Both test results show that the electrode material does not show the normal supercapacitor electrode material behavior of the β-MnO2@δ-MnO2 composite material. This is mainly due to the large difference in the morphology and size between β-MnO2 and δ-MnO2, which makes it impossible for δ-MnO2 to grow on the relatively smaller β-MnO2.
[0206] Test 6: Effect of different dosages of β-MnO2 nanorod material on the performance of the working electrode.
[0207] Table 1 The feeding conditions of different dosages of β-MnO2 nanorod materials
[0208]
[0209]
[0210] Table 2 Effect of different dosages of β-MnO2 nanorod materials on electrode performance
[0211] Active Materials <![CDATA[Electrochemical performance / F·g -1 > Rate performance / % Application Example 1 Example 1 132.4 74.2 Application Example 2 Example 2 103 61.8 Application Example 3 Example 3 95 50.1 Application Example 4 Example 4 99.8 72.2 Application Example 5 Example 5 129 51.3 Application Example 6 Example 6 124.4 61 Application Comparative Example 1 Comparative Example 1 12 69 Application Comparative Example 2 Comparative Example 2 62.3 43.5 Application Comparative Example 3 Comparative Example 5 120.5 55.5
[0212] Note: The rate performance is based on Figure 6 The capacitance retention of the electrode materials shown at different current densities; the cycle life is calculated based on Figure 7 The capacitance retention of the working electrode shown in the figure after 10,000 charge and discharge tests.
[0213] By analyzing the data in Table 2, it can be seen that compared with other embodiments and comparative examples, the β-MnO2@δ-MnO2 heterostructure material prepared in Example 1 is used as an active material to prepare a working electrode, and the electrochemical performance is the best, with the highest specific capacitance value and excellent rate performance. Later, the cycle stability is also tested, showing that under 10,000 cycles, its specific capacitance value can still maintain 97% of the initial value. This shows that the embodiment of the present invention uses the long chain structure of CTAB to promote the peeling and shedding of δ-MnO2 nanosheets through the mutual cooperation of appropriate amounts of β-MnO2 nanorod material, KMnO4 and CTAB, thereby controlling the size of δ-MnO2, realizing the vertical growth of ultra-thin layered δ-MnO2 nanosheets on solid β-MnO2 nanorods, and successfully preparing a β-MnO2@δ-MnO2 heterostructure material with stable structure, and exhibiting the best electrochemical performance at the ratio of Example 1.
[0214] Test 7: Effect of different hydrothermal temperatures on product purity
[0215] Table 3 Feeding conditions of different hydrothermal temperature experiments
[0216] Example 1 Example 7 Comparative Example 3 Comparative Example 4 Water temperature / ℃ 140 145 160 120
[0217] The screening test was conducted by regulating the hydrothermal temperature conditions of β-MnO2@δ-MnO2 heterostructure materials induced by using CTAB as one of the raw materials. By observing the SEM images during the test, it was found that when the temperature rose to 160°C, the generated MnO2 was not completely δ-MnO2, and part of it would become α-MnO2, because the most suitable growth temperature of δ-MnO2 was 140°C. Once it reached 160°C, a phase change would occur, and part of δ-MnO2 would be transformed into α-MnO2. When the temperature rose to 120°C, the generated MnO2 was not completely δ-MnO2, and there would be a large amount of potassium permanganate residue and unknown impurities. Moreover, when the hydrothermal temperature was higher than 140°C or lower than 140°C, the SEM images showed that more impurities appeared. It was determined that the most suitable reaction temperature for generating MnO2 using CTAB was 140°C.
[0218] Test 8: Effect of different hydrothermal reaction times on the electrochemical properties of the products
[0219] Fig. 9 It is an electron microscope scanning image of the β-MnO2@δ-MnO2 heterostructure material prepared at different hydrothermal reaction times in Examples 8-10. Fig. 9 (a) is an electron microscope scanning image of the material prepared in Example 8; (b) is an electron microscope scanning image of the material prepared in Example 9; (c) is an electron microscope scanning image of the material prepared in Example 10. Fig.10 It is a graph showing the electrochemical test results of the working electrodes prepared in Examples 7-9. Fig.10 (a) is a cyclic voltammetry (CV) test curve of the working electrode of Application Example 7; (b) is a constant current charge and discharge (GCD) curve of the working electrode of Application Example 7; (c) is a cyclic voltammetry (CV) test curve of the working electrode of Application Example 8; (d) is a constant current charge and discharge (GCD) curve of the working electrode of Application Example 8; (e) is a cyclic voltammetry (CV) test curve of the working electrode of Application Example 9; (f) is a constant current charge and discharge (GCD) curve of the working electrode of Application Example 9.
[0220] Table 4 Effect of different reaction times on the electrochemical properties of the products
[0221] Reaction time Working electrode <![CDATA[Electrochemical performance / F·g -1 > Example 1 12 Application Example 1 132.4 Example 8 16 Application Example 7 128.9 Example 9 20 Application Example 8 124.4 Example 10 24 Application Example 9 120.5
[0222] By controlling the reaction time, we can obtain the β-MnO2@δ-MnO2 heterostructure material with the best performance and morphology. We not only use 12h (the time used in the patent), but also use 16h, 20h, and 24h reaction time. Fig. 9 and Figure 2-3 From the SEM results, it can be seen that when the reaction time is 16h, 20h, and 24h, there is uneven growth. Compared with the heterogeneous structure materials generated at 16h, 20h, and 24h, the morphology of the β-MnO2@δ-MnO2 heterogeneous structure material generated at 12h is the most uniform.
[0223] pass Fig.10 and Figure 4-5 The electrochemical test results show that the working electrode of Example 1 is Figure 4 The cyclic voltammetry test curve of Figure 5 The charging and discharging branches of the supercapacitor exhibit triangular symmetry, showing the ideal behavior of supercapacitor electrode materials. Figure 5 The GCD results show that β-MnO2@δ-MnO2 at 1A·g -1 The specific capacitance is 132.4F·g -1 , which is much higher than the specific capacitance of traditional β-MnO2 (9F·g -1 ).
[0224] When the reaction time is 16h, 20h, and 24h, the growth is uneven, and the electrochemical performance is worse than that of 12h (132.4F·g -1 ) decreased, 16h(128.9F·g -1 ), 20h(124.4F·g -1), 24h(120.5F·g -1 ). Therefore, in comparison, the β-MnO2@δ-MnO2 heterostructure material generated under 12h has the best performance and the most uniform morphology.
[0225] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a β-MnO2@δ-MnO2 heterostructure material, characterized in that: The following steps are involved: Dissolve manganese sulfate and ammonium persulfate in water, and then conduct a hydrothermal reaction to obtain β-MnO2 nanomaterials; The β-MnO2 nanomaterial, potassium permanganate, CTAB and water are uniformly mixed, and then a secondary hydrothermal reaction is carried out to vertically grow ultra-thin layered δ-MnO2 nanosheets on solid β-MnO2 nanorods to obtain β-MnO2@δ-MnO2 heterostructure materials; The mass ratio of β-MnO2 nanomaterial to potassium permanganate and CTAB is 0.1-0.6:0.55-0.6:0.04; The temperature of the secondary hydrothermal reaction is 140~145°C; the time of the secondary hydrothermal reaction is 10~16h.
2. The method for preparing the β-MnO2@δ-MnO2 heterostructure material according to claim 1, characterized in that: The mass ratio of manganese sulfate to ammonium persulfate is 0.8~0.85:1.
1.
3. The method for preparing the β-MnO2@δ-MnO2 heterostructure material according to claim 1, characterized in that: The temperature of a hydrothermal reaction is 140~145°C; the time of a hydrothermal reaction is 10~16h.
4. The method for preparing the β-MnO2@δ-MnO2 heterostructure material according to claim 1, characterized in that: β-MnO2 nanomaterial is a nanorod structure material.
5. A β-MnO2@δ-MnO2 heterostructure material, characterized in that: The method is prepared by any one of claims 1 to 4.
6. Use of the β-MnO2@δ-MnO2 heterostructure material according to claim 5, characterized in that: The β-MnO2@δ-MnO2 heterostructure material is used as an active material for preparing a working electrode.
7. The use according to claim 6, characterized in that The working electrode is prepared by dispersing a binder, a conductive agent and an active material in an organic solvent to obtain a slurry, and then coating the slurry on a current collector.
8. The use according to claim 7, characterized in that The binder is PVDF; the conductive agent is acetylene black; the organic solvent is NMP; the current collector is carbon paper; the mass ratio of the binder, the conductive agent, and the active material is 0.005:0.005:0.
04.
9. The use according to claim 6, characterized in that: The β-MnO2@δ-MnO2 heterostructure material is used as an active material to prepare a working electrode of a supercapacitor.
Citation Information
Patent Citations
MnO2 nanometer composite material and preparation method thereof
CN103771524A
Rodlike manganese dioxide / polyaniline composite material as well as preparation method and application of rodlike manganese dioxide
CN106684331A
Lithium-rich manganese-based positive electrode material with lithium layer doped with divalent cations and preparation method of lithium-rich manganese-based positive electrode material
CN112897584A
Manganese-based positive electrode material of two-phase composite zinc ion battery and preparation method of manganese-based positive electrode material
CN113193189A
Preparation method of CTAB (Cetyltrimethyl Ammonium Bromide)-induced delta-MnO2 nanoflower supercapacitor positive electrode material as well as product and application thereof
CN114516660A