A filter element made of a stain-resistant material and a preparation method thereof
Through the multi-layer structure filter element design, the porous structure of composite fiber materials and nano-activated carbon is used to solve the problem of water purification agent detachment in the filter element, achieving high-efficiency filtration and long-term use, and improving the cleanliness and taste of water.
Patent Information
- Application Number
- CN202311570736.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-11-23
AI Technical Summary
During the use of the existing filter element, the loaded water purification agent is easy to detach, resulting in a reduction in purification effect, and cannot effectively solve the problem of water quality and taste and the long-term filtration effect of pollutants.
The filter element is designed with a multi-layer structure, in which the inner fine filter fiber layer is interwoven with composite fiber material and polytetrafluoroethylene fiber, the medium fine filter fiber layer and the outer coarse filter fiber layer are made of polyester fiber or nylon fiber, and the skeleton fiber layer Embedded with ion exchange resin particles and zeolite particles, through hydrothermal reaction and vacuum impregnation technology, a porous structure is formed to carry nano-activated carbon and titanium dioxide nanorods to enhance filtration precision and pollution resistance.
It achieves a stable load of nano activated carbon, improves the filtration effect and the pollution resistance of the filter element, extends the service life, and has a sterilization and decontamination effect under light, ensuring the cleanliness and taste of the water.
Smart Images

Figure GDA0004975440090000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of filter element materials, and in particular to a filter element made of a stain-resistant material and a preparation method thereof. Background Art
[0002] With the rapid development of industry, water, air and soil pollution are becoming increasingly serious. The quality of water sources in my country is deteriorating. Groundwater and shallow surface water in many cities are seriously polluted. The deterioration of water quality has aggravated the rapid development of the water purification market. Water treated by water purifiers basically meets the safety of drinking water. The water purifiers that use reverse osmosis purification in related technologies can remove most of the ions, minerals and organic matter in the water. The water quality is acidic and tastes green. Although it meets the needs of hygiene and safety, the taste of the water is greatly reduced, and the original refreshing and sweet characteristics of water are completely lost. As people's awareness of the safety and taste of drinking water increases, water with good taste is more and more favored by consumers.
[0003] For example, the invention patent with announcement number CN107285396A discloses a degradable PLA water purification filter element, the main material of the filter element is PLA fiber, the PLA fiber is made by blending PLLA, PDLA, PGLA and a water purifier, and then extruded from a spinneret at 160-200°C, and formed into a fiber web and molded by a rolling collector; the water purifier is one or more of nano zinc oxide, nano silver, and activated carbon; the filter element can achieve physical filtration while playing a relatively effective antibacterial and bactericidal role, and at the same time, after the PLA filter element is replaced, it can be completely degraded in a composting environment; however, during the use of the filter element, the water purifier loaded in the PLA fiber is easily detached under the action of water flow, resulting in a gradual reduction in the water purifier loaded in the PLA fiber, thereby affecting the purification effect. Summary of the invention
[0004] In view of the problems existing in the prior art, the object of the present invention is to provide a filter element made of a stain-resistant material and a preparation method thereof.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A filter element of a dirt-resistant material, the filter element is cylindrical and includes, from the inside to the outside in the radial direction, an inner fine filter fiber layer, an adsorbent fiber layer, a medium and fine filter fiber layer, a skeleton fiber layer and an outer coarse filter fiber layer, wherein the filter aperture of each layer of the inner fine filter fiber layer, the medium and fine filter fiber layer and the outer coarse filter fiber layer increases in a gradually sparse gradient from the inside to the outside in the radial direction;
[0007] The inner fine filter fiber layer is composed of a composite fiber material and polytetrafluoroethylene fibers interwoven together;
[0008] The composite fiber material uses porous carbon fibers as a matrix, loads nanorods through a hydrothermal reaction, and obtains composite porous carbon fibers. Then, the nano activated carbon is infiltrated into the voids of the composite porous carbon fibers through vacuum impregnation to obtain the composite fiber material.
[0009] As a further preferred embodiment of the present invention, the absorbent fiber layer is composed of carbon fiber or plant fiber;
[0010] The medium fine filter fiber layer and the outer coarse filter fiber layer are composed of polyester fibers or nylon fibers;
[0011] The skeleton fiber layer is composed of glass fiber or polyethylene fiber.
[0012] As a further preferred embodiment of the present invention, an active agent is embedded in the skeleton fiber layer and the outer coarse filter fiber layer, and the active agent is a mixture of ion exchange resin particles and zeolite particles in a weight ratio of 1:(1-2), and the ion exchange resin particles are a mixture of anion exchange resin particles and cation exchange resin particles in a weight ratio of 1:(2-4).
[0013] As a further preferred embodiment of the present invention, the preparation method of the composite porous carbon fiber is as follows:
[0014] 1) Adding polyacrylonitrile powder and dimethyl sulfoxide to a container in sequence, stirring evenly at 60-65° C. to prepare a solution, then adding potassium carbonate to the solution and continuing to stir for 5-10 hours, mixing evenly to obtain a spinning solution, then extruding the spinning solution into a 55-58° C. potassium carbonate aqueous solution at a pressure of 0.3-0.8 MPa for coagulation, and placing the coagulated fiber in a 60-70° C. vacuum drying oven for 45-50 hours to obtain a polypropylene fiber;
[0015] 2) placing the polypropylene fiber in an oven, treating it at 180-190° C. and 230-240° C. for 10-20 min and 30-50 min respectively, then transferring it to a crucible, treating it at 800-850° C. for 1-3 h in a nitrogen atmosphere, cooling it naturally to room temperature after the treatment, repeatedly washing it with a hydrochloric acid solution, and drying it to obtain a porous carbon fiber;
[0016] 3) Dissolve polyvinyl pyrrolidone in 1-pentanol, then add sodium citrate solution and stir thoroughly to dissolve, then add deionized water, concentrated hydrochloric acid and tetrabutyl titanate in sequence, stir thoroughly to dissolve to obtain a titanium dioxide source solution, then immerse the porous carbon fiber in the titanium dioxide source solution, transfer it to a reactor, seal it, and perform a hydrothermal reaction at 90-120°C for 15-25h. After the reaction is completed, wash the product repeatedly with deionized water and anhydrous ethanol, and blow dry it with nitrogen to obtain a composite porous carbon fiber.
[0017] As a further preferred embodiment of the present invention, in step 1), the solid content of the solution is 20-25wt%;
[0018] The amount of potassium carbonate added is 1-5% of the mass of polyacrylonitrile;
[0019] The concentration of the potassium carbonate aqueous solution is 1-5 wt %.
[0020] As a further preferred embodiment of the present invention, in step 2), the flow rate of the nitrogen is 1.0-1.6 L / min.
[0021] As a further preferred embodiment of the present invention, in step 3), the usage ratio of polyvinyl pyrrolidone, 1-pentanol, sodium citrate solution, deionized water, concentrated hydrochloric acid, and tetrabutyl titanate is (0.5-1.0) g: (5-10) mL: (100-200) μL: (5-13) mL: (5-10) mL: (200-300) μL;
[0022] The concentration of the sodium citrate solution is 0.3-0.5 mol / L;
[0023] The concentration of the concentrated hydrochloric acid is 12-14 mol / L;
[0024] The added amount of the porous carbon fiber is 3-8% of the total mass of the titanium dioxide source solution.
[0025] As a further preferred embodiment of the present invention, the preparation method of the composite fiber material is as follows:
[0026] 1) Dry the high carbon ash at 105-115° C. for 2-5 h, grind it into fine powder, mix it with potassium hydroxide of equal mass, transfer it to a reactor, heat it to 1200-1300° C. in a nitrogen atmosphere, keep it warm for 1-3 h, cool it to room temperature after the treatment, pickle it with a hydrochloric acid solution with a concentration of 10-13wt%, wash it repeatedly with deionized water until it is neutral, dry it, grind it, and obtain activated nano activated carbon;
[0027] 2) Dispersing the activated nano-activated carbon in deionized water to obtain a dispersion, then placing the composite porous carbon fiber in a vacuum impregnator, evacuating to 50-100Pa, maintaining for 5-10min, then injecting a sufficient amount of the dispersion, and evacuating to 10-30Pa, continuing to maintain for 20-40min, slowly releasing the pressure to normal pressure, repeating the operation 2-5 times, and drying after centrifugal separation to obtain a composite fiber material.
[0028] As a further preferred embodiment of the present invention, the heating rate under the nitrogen atmosphere is 10-20°C / min;
[0029] The concentration of the dispersion is 3-8 wt %.
[0030] A method for preparing a filter element made of a stain-resistant material comprises the following steps:
[0031] The composite fiber material and polytetrafluoroethylene fiber are alternately hot-melt-spinned and wound into a cylindrical inner fine filter fiber layer, an adsorbent fiber layer is wound on the inner fine filter fiber layer, a medium and fine filter fiber layer is wound on the adsorbent fiber layer, a skeleton fiber layer is wound on the medium and fine filter fiber layer, and an outer coarse filter fiber layer is wound on the skeleton fiber layer.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] In the present invention, potassium carbonate is used as an additive to obtain polypropylene fiber through wet spinning, and then a porous carbon fiber with a porous structure is obtained through simultaneous carbonization and activation. Then, the porous carbon fiber is used as a carrier, and a large number of titanium dioxide nanorods are deposited in the porous carbon fiber through a microemulsion hydrothermal method, so as to obtain a composite porous carbon fiber, whose rich pore structure provides sufficient places for the deposition of titanium dioxide nanorods. The deposited titanium dioxide nanorods are stacked with each other to form a cross skeleton structure, which can support the voids of the composite porous carbon fiber on the one hand, avoid the phenomenon of pore collapse in the subsequent vacuum impregnation process, thereby facilitating the subsequent vacuum impregnation, so that the nano activated carbon can be smoothly infiltrated into the pores, and on the other hand, the skeleton structure formed in the pores increases the meandering tortuosity of the pores, thereby extending the moving path of the subsequently infiltrated nano activated carbon and the friction resistance, so as to effectively prevent the loss of the nano activated carbon and achieve the stability of the nano activated carbon load.
[0034] In the present invention, high carbon ash is used as raw material, and potassium hydroxide is used for high-temperature alkali activation treatment, so that the original pore structure in the fine ash collapses, the carbon skeleton structure breaks, and more microporous structures are generated. Through subsequent acid washing, the pores blocked in the reaction process can be unblocked, so that nano-activated carbon with high porosity can be obtained, and then the nano-activated carbon is infiltrated into the composite porous carbon fiber by vacuum impregnation, so as to obtain a composite fiber material. The composite fiber material has a rich microporous structure inside, and under the action of capillaries, extremely small particles and bacteria in the filter medium can be filtered out, thereby ensuring the cleanliness of the filter medium and improving the filtering effect. Moreover, the titanium dioxide nanorods loaded in the composite fiber material have a good sterilization and decontamination effect under light, so that the filtered bacteria and dirt can be efficiently removed, thereby improving the cleanliness of the composite fiber material, allowing it to be repeatedly used, thereby improving its anti-fouling performance.
[0035] The filter element in the present invention is composed of multiple layers of fibers, and the filter aperture gradually increases from the inside to the outside, thereby increasing the filter area and the amount of dirt holding, having high filtration accuracy, good filtration effect, and greatly extending the service life. The innermost inner fine filter fiber layer is composed of a composite fiber material and polytetrafluoroethylene fibers interwoven together, wherein the polytetrafluoroethylene fibers have high strength and high elongation, good stability, and are used in combination with the composite fiber material to have excellent mechanical properties and dirt resistance, thereby achieving efficient filtration effects and a long service life. DETAILED DESCRIPTION
[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] In the embodiment of the present invention, the adsorptive fiber layer is composed of carbon fiber; the medium and fine filter fiber layer and the outer coarse filter fiber layer are composed of polyester fiber; and the skeleton fiber layer is composed of glass fiber.
[0038] Active agents are embedded in the skeleton fiber layer and the outer coarse filter fiber layer. The active agent is a mixture of ion exchange resin particles and zeolite particles in a weight ratio of 1:2, and the ion exchange resin particles are a mixture of anion exchange resin particles and cation exchange resin particles in a weight ratio of 1:3. The anion exchange resin is AMBERJET 4200Cl anion exchange resin from Dow Rohm and Haas of the United States, and the cation exchange resin is C100E cation exchange resin from Purolite of the United Kingdom.
[0039] Example 1
[0040] A filter element of a dirt-resistant material, the filter element is cylindrical and includes, from the inside to the outside in the radial direction, an inner fine filter fiber layer, an adsorbent fiber layer, a medium and fine filter fiber layer, a skeleton fiber layer and an outer coarse filter fiber layer, wherein the filter aperture of each layer of the inner fine filter fiber layer, the medium and fine filter fiber layer and the outer coarse filter fiber layer increases in a gradually sparse gradient from the inside to the outside in the radial direction;
[0041] The inner fine filter fiber layer is composed of composite fiber material and polytetrafluoroethylene fiber interwoven;
[0042] The composite fiber material is based on porous carbon fiber as the matrix, and nanorods are loaded after hydrothermal reaction to obtain composite porous carbon fiber. Then, the nano activated carbon is infiltrated into the voids of the composite porous carbon fiber by vacuum impregnation to obtain the composite fiber material.
[0043] The preparation method of the filter element specifically comprises the following steps:
[0044] The composite fiber material and polytetrafluoroethylene fiber are alternately hot-melt-spinned and wound into a cylindrical inner fine filter fiber layer, an adsorbent fiber layer is wound on the inner fine filter fiber layer, a medium and fine filter fiber layer is wound on the adsorbent fiber layer, a skeleton fiber layer is wound on the medium and fine filter fiber layer, and an outer coarse filter fiber layer is wound on the skeleton fiber layer.
[0045] Wherein, the preparation method of the composite fiber material is as follows:
[0046] 1) polyacrylonitrile powder and dimethyl sulfoxide are added to a container in sequence, stirred evenly at 60° C. to prepare a solution with a solid content of 20 wt%, then potassium carbonate is added to the solution and stirred for 5 hours, wherein the amount of potassium carbonate added is 1% of the mass of polyacrylonitrile, and the spinning solution is obtained after uniform mixing, and then the spinning solution is extruded into a 1 wt % potassium carbonate aqueous solution at 55° C. under a pressure of 0.3 MPa for coagulation, and the coagulated fiber is placed in a vacuum drying oven at 60° C. and dried for 45 hours to obtain polypropylene fiber;
[0047] 2) placing the polypropylene fiber in an oven, treating it at 180°C and 230°C for 10 min and 30 min respectively, then transferring it to a crucible, treating it at 800°C for 1 h in a nitrogen atmosphere, with a nitrogen flow rate of 1.0 L / min, cooling it naturally to room temperature after the treatment, repeatedly washing it with a hydrochloric acid solution, and drying it to obtain a porous carbon fiber;
[0048] 3) 0.5g of polyvinyl pyrrolidone was dissolved in 5mL of 1-pentanol, and then 100μL of a sodium citrate solution with a concentration of 0.3mol / L was added, and the mixture was fully stirred and dissolved. Then, 5mL of deionized water, 5mL of concentrated hydrochloric acid with a concentration of 12mol / L, and 200μL of tetrabutyl titanate were added in sequence, and the titanium dioxide source solution was obtained after sufficient stirring and dissolution. The porous carbon fiber was then immersed in the titanium dioxide source solution, and the amount of the porous carbon fiber added was controlled to be 3% of the total mass of the titanium dioxide source solution. The mixture was then transferred to a reactor, sealed, and subjected to a hydrothermal reaction at 90°C for 15h. After the reaction was completed, the product was repeatedly washed with deionized water and anhydrous ethanol, and dried with nitrogen to obtain a composite porous carbon fiber.
[0049] 4) Dry the high carbon ash at 105°C for 2h, grind it into fine powder, mix it with potassium hydroxide of equal mass, transfer it to a reactor, heat it to 1200°C at a rate of 10°C / min under a nitrogen atmosphere, keep it warm for 1h, cool it to room temperature after the treatment, pickle it with a 10wt% hydrochloric acid solution, wash it repeatedly with deionized water until it is neutral, dry it, grind it, and obtain activated nano-activated carbon;
[0050] 5) The activated nano-activated carbon is dispersed in deionized water to obtain a dispersion with a concentration of 3wt%, and then the composite porous carbon fiber is placed in a vacuum impregnator, evacuated to 50Pa, maintained for 5min, and then a sufficient amount of the dispersion is injected, and evacuated to 10Pa, and maintained for 20min, and then the pressure is slowly released to normal pressure. The operation is repeated twice, and after centrifugal separation and drying, a composite fiber material can be obtained.
[0051] Example 2
[0052] A filter element of a dirt-resistant material, the filter element is cylindrical and includes, from the inside to the outside in the radial direction, an inner fine filter fiber layer, an adsorbent fiber layer, a medium and fine filter fiber layer, a skeleton fiber layer and an outer coarse filter fiber layer, wherein the filter aperture of each layer of the inner fine filter fiber layer, the medium and fine filter fiber layer and the outer coarse filter fiber layer increases in a gradually sparse gradient from the inside to the outside in the radial direction;
[0053] The inner fine filter fiber layer is composed of composite fiber material and polytetrafluoroethylene fiber interwoven;
[0054] The composite fiber material is based on porous carbon fiber as the matrix, and nanorods are loaded after hydrothermal reaction to obtain composite porous carbon fiber. Then, the nano activated carbon is infiltrated into the voids of the composite porous carbon fiber by vacuum impregnation to obtain the composite fiber material.
[0055] The preparation method of the filter element specifically comprises the following steps:
[0056] The composite fiber material and polytetrafluoroethylene fiber are alternately hot-melt-spinned and wound into a cylindrical inner fine filter fiber layer, an adsorbent fiber layer is wound on the inner fine filter fiber layer, a medium and fine filter fiber layer is wound on the adsorbent fiber layer, a skeleton fiber layer is wound on the medium and fine filter fiber layer, and an outer coarse filter fiber layer is wound on the skeleton fiber layer.
[0057] Wherein, the preparation method of the composite fiber material is as follows:
[0058] 1) polyacrylonitrile powder and dimethyl sulfoxide are added to a container in sequence, stirred evenly at 63° C. to prepare a solution with a solid content of 23 wt%, then potassium carbonate is added to the solution and stirred for 7 hours, wherein the amount of potassium carbonate added is 3% of the mass of polyacrylonitrile, and the spinning solution is obtained after uniform mixing, and then the spinning solution is extruded into a 3 wt % potassium carbonate aqueous solution at 56° C. under a pressure of 0.5 MPa for coagulation, and the coagulated fiber is placed in a vacuum drying oven at 65° C. and dried for 48 hours to obtain polypropylene fiber;
[0059] 2) placing the polypropylene fiber in an oven, treating it at 185°C and 235°C for 15 min and 40 min respectively, then transferring it to a crucible, treating it at 830°C for 2 h in a nitrogen atmosphere, with a nitrogen flow rate of 1.3 L / min, cooling it naturally to room temperature after the treatment, repeatedly washing it with a hydrochloric acid solution, and drying it to obtain a porous carbon fiber;
[0060] 3) 0.7 g of polyvinyl pyrrolidone was dissolved in 7 mL of 1-pentanol, and then 150 μL of a sodium citrate solution with a concentration of 0.4 mol / L was added, and the solution was fully stirred and dissolved, and then 10 mL of deionized water, 8 mL of concentrated hydrochloric acid with a concentration of 13 mol / L, and 260 μL of tetrabutyl titanate were added in sequence, and the titanium dioxide source solution was obtained after sufficient stirring and dissolution, and then the porous carbon fiber was immersed in the titanium dioxide source solution, and the amount of porous carbon fiber added was controlled to be 5% of the total mass of the titanium dioxide source solution, and then transferred to a reactor, sealed, and hydrothermally reacted at 110° C. for 20 h. After the reaction was completed, the product was repeatedly washed with deionized water and anhydrous ethanol, and dried with nitrogen to obtain a composite porous carbon fiber;
[0061] 4) Dry the high carbon ash at 110° C. for 3 h, grind it into fine powder, mix it with an equal mass of potassium hydroxide, transfer it to a reactor, heat it to 1250° C. at a rate of 15° C. / min under a nitrogen atmosphere, keep it warm for 2 h, cool it to room temperature after the treatment is completed, pickle it with a 12wt% hydrochloric acid solution, wash it repeatedly with deionized water until it is neutral, dry it, grind it, and obtain activated nano-activated carbon;
[0062] 5) The activated nano-activated carbon is dispersed in deionized water to obtain a dispersion with a concentration of 5 wt%, and then the composite porous carbon fiber is placed in a vacuum impregnator, evacuated to 70 Pa, maintained for 7 min, and then a sufficient amount of the dispersion is injected, and evacuated to 20 Pa, and maintained for 30 min, and then the pressure is slowly released to normal pressure. The operation is repeated 3 times, and after centrifugal separation and drying, a composite fiber material can be obtained.
[0063] Example 3
[0064] A filter element of a dirt-resistant material, the filter element is cylindrical and includes, from the inside to the outside in the radial direction, an inner fine filter fiber layer, an adsorbent fiber layer, a medium and fine filter fiber layer, a skeleton fiber layer and an outer coarse filter fiber layer, wherein the filter aperture of each layer of the inner fine filter fiber layer, the medium and fine filter fiber layer and the outer coarse filter fiber layer increases in a gradually sparse gradient from the inside to the outside in the radial direction;
[0065] The inner fine filter fiber layer is composed of composite fiber material and polytetrafluoroethylene fiber interwoven;
[0066] The composite fiber material is based on porous carbon fiber as the matrix, and nanorods are loaded after hydrothermal reaction to obtain composite porous carbon fiber. Then, the nano activated carbon is infiltrated into the voids of the composite porous carbon fiber by vacuum impregnation to obtain the composite fiber material.
[0067] The preparation method of the filter element specifically comprises the following steps:
[0068] The composite fiber material and polytetrafluoroethylene fiber are alternately hot-melt-spinned and wound into a cylindrical inner fine filter fiber layer, an adsorbent fiber layer is wound on the inner fine filter fiber layer, a medium and fine filter fiber layer is wound on the adsorbent fiber layer, a skeleton fiber layer is wound on the medium and fine filter fiber layer, and an outer coarse filter fiber layer is wound on the skeleton fiber layer.
[0069] Wherein, the preparation method of the composite fiber material is as follows:
[0070] 1) polyacrylonitrile powder and dimethyl sulfoxide are added to a container in sequence, stirred evenly at 65° C. to prepare a solution with a solid content of 25 wt%, then potassium carbonate is added to the solution and stirred for 10 hours, wherein the amount of potassium carbonate added is 5% of the mass of polyacrylonitrile, and the spinning solution is obtained after uniform mixing, and then the spinning solution is extruded into a 5 wt % potassium carbonate aqueous solution at 58° C. under a pressure of 0.8 MPa for coagulation, and the coagulated fiber is placed in a vacuum drying oven at 70° C. and dried for 50 hours to obtain a polypropylene fiber;
[0071] 2) placing the polypropylene fiber in an oven, treating it at 190°C and 240°C for 20 min and 50 min respectively, then transferring it to a crucible, treating it at 850°C for 3 h in a nitrogen atmosphere, with a nitrogen flow rate of 1.6 L / min, cooling it naturally to room temperature after the treatment, repeatedly washing it with a hydrochloric acid solution, and drying it to obtain a porous carbon fiber;
[0072] 3) 1.0g polyvinyl pyrrolidone was dissolved in 10mL 1-pentanol, and then 200μL of 0.5mol / L sodium citrate solution was added, and the mixture was fully stirred and dissolved. Then 13mL deionized water, 10mL of 14mol / L concentrated hydrochloric acid and 300μL of tetrabutyl titanate were added in sequence, and the titanium dioxide source solution was obtained after full stirring and dissolution. The porous carbon fiber was then immersed in the titanium dioxide source solution, and the amount of the porous carbon fiber added was controlled to be 8% of the total mass of the titanium dioxide source solution. The mixture was then transferred to a reactor, sealed, and subjected to hydrothermal reaction at 120°C for 25h. After the reaction was completed, the product was repeatedly washed with deionized water and anhydrous ethanol, and dried with nitrogen to obtain a composite porous carbon fiber.
[0073] 4) Dry the high carbon ash at 115° C. for 5 h, grind it into fine powder, mix it with potassium hydroxide of equal mass, transfer it to a reactor, heat it to 1300° C. at a rate of 20° C. / min under a nitrogen atmosphere, keep it warm for 3 h, cool it to room temperature after the treatment, pickle it with a 13wt% hydrochloric acid solution, wash it repeatedly with deionized water until it is neutral, dry it, grind it, and obtain activated nano-activated carbon;
[0074] 5) The activated nano-activated carbon is dispersed in deionized water to obtain a dispersion with a concentration of 8 wt%, and then the composite porous carbon fiber is placed in a vacuum impregnator, evacuated to 100 Pa, maintained for 10 min, and then a sufficient amount of the dispersion is injected, and evacuated to 30 Pa, and continued to maintain for 40 min, and then the pressure is slowly released to normal pressure. The operation is repeated 5 times, and after centrifugal separation and drying, a composite fiber material can be obtained.
[0075] Comparative Example 1: This comparative example is basically the same as Example 1, except that the inner fine filter fiber layer does not contain composite fiber material.
[0076] Comparative Example 2: This comparative example is basically the same as Example 1, except that potassium carbonate in step 1) is omitted in the preparation of the composite fiber material.
[0077] Comparative Example 3: This comparative example is basically the same as Example 1, except that step 2) is omitted in the preparation of the composite fiber material.
[0078] Comparative Example 4: This comparative example is basically the same as Example 1, except that step 3) is omitted in the preparation of the composite fiber material.
[0079] Comparative Example 5: This comparative example is basically the same as Example 1, except that, in the preparation of the composite fiber material, step 4) is omitted and nano-grade activated carbon is used instead of activated nano-activated carbon.
[0080] Test experiment:
[0081] The composite fiber material samples provided in Examples 1-3 and Comparative Examples 1-5 were respectively used and interwoven with polytetrafluoroethylene fibers to form an inner fine filter fiber layer. The initial stain resistance and stain resistance after 50 washes were measured according to the standard AATCC130:2010 "Test Method for Stain Removal Performance of Textiles". The test results are shown in Table 1.
[0082] Table 1
[0083]
[0084] It can be seen from Table 1 that the inner fine filter fiber layer in the present invention has good stain resistance, and the filter element processed and manufactured has a high-efficiency filtering effect and a long service life.
[0085] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing a filter element of a stain-resistant material, characterized in that: The filter element is cylindrical and includes an inner fine filter fiber layer, an adsorbent fiber layer, a medium fine filter fiber layer, a skeleton fiber layer and an outer coarse filter fiber layer in order from the inside to the outside in the radial direction, wherein the filter aperture of each layer of the inner fine filter fiber layer, the medium fine filter fiber layer and the outer coarse filter fiber layer increases gradually from the inside to the outside in the radial direction; The inner fine filter fiber layer is composed of a composite fiber material and polytetrafluoroethylene fibers interwoven together; The composite fiber material is a composite porous carbon fiber that is loaded with nanorods after a hydrothermal reaction to obtain a composite porous carbon fiber, and then activated nano activated carbon is infiltrated into the voids of the composite porous carbon fiber by vacuum impregnation to obtain the composite fiber material. The preparation method of the composite porous carbon fiber is as follows: 1) Adding polyacrylonitrile powder and dimethyl sulfoxide to a container in sequence, stirring evenly at 60-65° C. to prepare a solution, then adding potassium carbonate to the solution and continuing to stir for 5-10 hours, mixing evenly to obtain a spinning solution, then extruding the spinning solution into a 55-58° C. potassium carbonate aqueous solution at a pressure of 0.3-0.8 MPa for coagulation, and placing the coagulated fiber in a 60-70° C. vacuum drying oven for 45-50 hours to obtain a polypropylene fiber; 2) placing the polypropylene fiber in an oven, treating it at 180-190° C. and 230-240° C. for 10-20 min and 30-50 min respectively, then transferring it to a crucible, treating it at 800-850° C. for 1-3 h in a nitrogen atmosphere, cooling it naturally to room temperature after the treatment, repeatedly washing it with a hydrochloric acid solution, and drying it to obtain a porous carbon fiber; 3) dissolving polyvinyl pyrrolidone in 1-pentanol, then adding sodium citrate solution, stirring and dissolving, then adding deionized water, concentrated hydrochloric acid and tetrabutyl titanate in sequence, stirring and dissolving to obtain a titanium dioxide source solution, then immersing the porous carbon fiber in the titanium dioxide source solution, transferring it to a reactor, sealing it, and performing a hydrothermal reaction at 90-120° C. for 15-25 hours. After the reaction is completed, the product is repeatedly washed with deionized water and anhydrous ethanol, and dried with nitrogen to obtain a composite porous carbon fiber; In step 1), the solid content of the solution is 20-25wt%; The amount of potassium carbonate added is 1-5% of the mass of polyacrylonitrile; The concentration of the potassium carbonate aqueous solution is 1-5wt%; In step 2), the flow rate of the nitrogen is 1.0-1.6 L / min; In step 3), the usage ratio of polyvinyl pyrrolidone, 1-pentanol, sodium citrate solution, deionized water, concentrated hydrochloric acid, and tetrabutyl titanate is (0.5-1.0) g: (5-10) mL: (100-200) μL: (5-13) mL: (5-10) mL: (200-300) μL; The concentration of the sodium citrate solution is 0.3-0.5 mol / L; The concentration of the concentrated hydrochloric acid is 12-14 mol / L; The amount of the porous carbon fiber added is 3-8% of the total mass of the titanium dioxide source solution; The preparation method of the composite fiber material is as follows: 1) Dry the high carbon ash at 105-115° C. for 2-5 h, grind it into fine powder, mix it with potassium hydroxide of equal mass, transfer it to a reactor, heat it to 1200-1300° C. in a nitrogen atmosphere, keep it warm for 1-3 h, cool it to room temperature after the treatment, pickle it with a hydrochloric acid solution with a concentration of 10-13wt%, wash it repeatedly with deionized water until it is neutral, dry it, grind it, and obtain activated nano activated carbon; 2) Dispersing the activated nano-activated carbon in deionized water to obtain a dispersion, then placing the composite porous carbon fiber in a vacuum impregnator, evacuating to 50-100Pa, maintaining for 5-10min, then injecting a sufficient amount of the dispersion, and evacuating to 10-30Pa, continuing to maintain for 20-40min, slowly releasing the pressure to normal pressure, repeating the operation 2-5 times, and drying after centrifugal separation to obtain a composite fiber material.
2. The method for preparing a filter element made of a stain-resistant material according to claim 1, characterized in that: The absorbent fiber layer is composed of carbon fiber or plant fiber; The medium fine filter fiber layer and the outer coarse filter fiber layer are composed of polyester fibers or nylon fibers; The skeleton fiber layer is composed of glass fiber or polyethylene fiber.
3. The method for preparing a filter element made of a stain-resistant material according to claim 1, characterized in that: The skeleton fiber layer and the outer coarse filter fiber layer are embedded with an active agent, wherein the active agent is a mixture of ion exchange resin particles and zeolite particles in a weight ratio of 1:(1-2), and the ion exchange resin particles are a mixture of anion exchange resin particles and cation exchange resin particles in a weight ratio of 1:(2-4).
4. The method for preparing a filter element made of a stain-resistant material according to claim 1, characterized in that: In the nitrogen atmosphere, the heating rate is 10-20°C / min; The concentration of the dispersion is 3-8 wt %.
5. The method for preparing a filter element made of a stain-resistant material according to claim 1, characterized in that: The specific steps include: The composite fiber material and polytetrafluoroethylene fiber are alternately hot-melt-spinned and wound into a cylindrical inner fine filter fiber layer, an adsorbent fiber layer is wound on the inner fine filter fiber layer, a medium and fine filter fiber layer is wound on the adsorbent fiber layer, a skeleton fiber layer is wound on the medium and fine filter fiber layer, and an outer coarse filter fiber layer is wound on the skeleton fiber layer.