Single crystal diamond epitaxial wafer and preparation method thereof

By growing a doping layer on the seed layer of a single crystal diamond substrate and using substitutional impurities to repel other impurities, the problems of existing single crystal diamond substrates with high impurities and high surface roughness are solved, and high-quality single crystals are achieved. Diamond substrate preparation improves yield and performance.

CN117535793BActive Publication Date: 2024-10-11深圳平湖实验室
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311636178.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-30
Publication Date
2024-10-11
Estimated Expiration
2043-11-30

AI Technical Summary

Technical Problem

The existing single crystal diamond substrate has many impurities, high surface roughness and poor crystal plane orientation consistency, which limits the development of diamond in semiconductor devices and other application fields.

Method used

By growing a doping layer on the seed layer, and adding substitutional impurities to the doping layer to repel other impurities, an epitaxial layer with less impurities, small surface roughness and high consistency of crystal plane orientation is grown, forming a high-quality single crystal diamond substrate.

Benefits of technology

It significantly improves the yield of single crystal diamond substrates, reduces manufacturing costs, and improves the performance and reliability of diamond in application fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117535793B_ABST
    Figure CN117535793B_ABST
Patent Text Reader

Abstract

The present disclosure provides a single crystal diamond epitaxial wafer and a method for preparing the same, a substrate for growing a diamond epitaxial layer, and a method for preparing a single crystal diamond substrate, which relates to the technical field of semiconductor materials and aims to solve the problem that the existing single crystal diamond substrate has many impurities and high surface roughness. The single crystal diamond epitaxial wafer comprises: a seed layer and at least one group of stacked structures grown on the seed layer, the stacked structure comprising: a doped layer and an epitaxial layer stacked along a first direction, the material of the doped layer is a single crystal diamond containing a first impurity, the first impurity is a substitutional impurity in the doped layer, and the material of the epitaxial layer comprises single crystal diamond; wherein the first direction is a direction perpendicular to the seed layer and away from the seed layer. The above-mentioned single crystal diamond epitaxial wafer is used to prepare a single crystal diamond substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of semiconductor materials, and in particular to a single crystal diamond epitaxial wafer and a preparation method thereof, a substrate for growing a diamond epitaxial layer, and a preparation method of a single crystal diamond substrate. Background Art

[0002] Diamond is known as the "ultimate semiconductor" material, with many excellent properties, such as large bandgap, large hole and electron mobility, effective radiation resistance, etc. These excellent properties make diamond material have great potential in many application fields. With the development of semiconductor devices, microelectronics, nuclear energy and aerospace, the demand for large-scale single crystal diamond is becoming more and more urgent, and natural diamond is far from meeting people's needs. Summary of the invention

[0003] The embodiments of the present disclosure provide a single crystal diamond epitaxial wafer and a method for preparing the same, a substrate for growing a diamond epitaxial layer, and a method for preparing a single crystal diamond substrate, aiming to solve the problems of existing single crystal diamond substrates having many impurities, high surface roughness, and poor consistency of crystal orientation, so as to provide high-quality single crystal diamond substrates.

[0004] To achieve the above objectives, the embodiments of the present disclosure adopt the following technical solutions:

[0005] On the one hand, a single crystal diamond epitaxial wafer is provided, comprising: a seed layer and at least one group of stacked structures grown on the seed layer, the stacked structure comprising: a doped layer and an epitaxial layer stacked along a first direction, the material of the doped layer is single crystal diamond containing a first impurity, the first impurity is a substitutional impurity in the doped layer, and the material of the epitaxial layer comprises single crystal diamond; wherein the first direction is a direction perpendicular to the seed layer and away from the seed layer.

[0006] The embodiments of the present disclosure first grow a doped layer on a seed layer, wherein the doped layer is doped with a first impurity, and the first impurity is a substitutional impurity. The first impurity can exclude the content of other impurities that affect the quality of the crystal, thereby obtaining a doped layer with improved quality, and then grow an epitaxial layer, which is conducive to forming a high-quality epitaxial layer with less impurities, small surface roughness and high consistency of crystal orientation, so as to obtain a high-quality single crystal diamond substrate.

[0007] In some embodiments, the surface roughness of the doping layer is lower than the surface roughness of the seed layer; and / or the impurity concentration of the doping layer is lower than the impurity concentration of the seed layer.

[0008] In some embodiments, the consistency of the crystal plane orientation of the epitaxial layer is equal to that of the doped layer; and / or the surface roughness of the epitaxial layer is equal to that of the doped layer.

[0009] In some embodiments, the first impurity includes sulfur.

[0010] In some embodiments, the doping concentration of the first impurity is in the range of 10 16 / cm 3 ~10 17 / cm 3 .

[0011] In some embodiments, in a group of the stacked structures, the thickness of the epitaxial layer is greater than the thickness of the doped layer.

[0012] In some embodiments, the single crystal diamond epitaxial wafer comprises: at least two groups of the stacked structures, in which the doped layer is the first doped layer, the epitaxial layer is the first epitaxial layer, the remaining doped layers are the second doped layers, and the remaining epitaxial layers are the second epitaxial layers. The impurity concentration of the first doped layer is lower than the impurity concentration of the second doped layer; and / or, the surface roughness of the first doped layer is lower than the surface roughness of the second doped layer; and / or, the impurity concentration of the first epitaxial layer is lower than the impurity concentration of the second epitaxial layer; and / or, the surface roughness of the first epitaxial layer is lower than the surface roughness of the second epitaxial layer.

[0013] On the other hand, a substrate for growing a diamond epitaxial layer is provided, the substrate comprising: a seed layer and at least one doping layer grown on one side of the seed layer; the material of the doping layer is single crystal diamond containing a first impurity, and the first impurity is a substitutional impurity in the doping layer.

[0014] In some embodiments, the surface roughness of the doping layer is lower than the surface roughness of the seed layer; and / or the impurity concentration of the doping layer is lower than the impurity concentration of the seed layer.

[0015] In some embodiments, the number of the doped layers is at least two; the diamond epitaxial layer growth substrate further includes: at least one epitaxial layer, and the epitaxial layer is located between two adjacent doped layers.

[0016] It can be understood that the beneficial effects that can be achieved by the substrate for growing a diamond epitaxial layer provided in the above embodiments of the present disclosure can refer to the beneficial effects of the single crystal diamond epitaxial wafer mentioned above, and will not be repeated here.

[0017] On the other hand, a method for preparing a single crystal diamond epitaxial wafer is provided, the method comprising: providing a seed layer; growing a doping layer on the seed layer; the material of the doping layer is single crystal diamond containing a first impurity, and the first impurity is a substitutional impurity in the doping layer; growing an epitaxial layer on the doping layer; the material of the epitaxial layer comprises single crystal diamond.

[0018] In some embodiments, the method for preparing a single crystal diamond epitaxial wafer further includes: if the quality parameters of the epitaxial layer do not meet a preset target, returning to execute the step of growing the doped layer and the step of growing the epitaxial layer until the quality parameters of the epitaxial layer meet the preset target; the quality parameters of the epitaxial layer include at least one of impurities and surface roughness; and / or, if the epitaxial layer does not meet a thickness parameter target, returning to execute the step of growing the epitaxial layer until the epitaxial layer meets the thickness parameter target.

[0019] In some embodiments, when the quality parameters of the epitaxial layer include impurities, the preset targets include: the Raman spectrum of the epitaxial layer has no impurity characteristic peaks, and the impurity characteristic peaks are characteristic peaks outside the diamond phase; when the quality parameters of the epitaxial layer include surface roughness, the preset targets include: the surface roughness of the epitaxial layer is less than the surface roughness of the seed crystal layer; the thickness parameter target of the epitaxial layer includes the thickness range of the epitaxial layer being 500μm to 5000μm.

[0020] In some embodiments, growing a doped layer on the seed layer includes: reacting a first growth gas with a doping source gas in an environment of a first carrier gas to obtain a doped layer grown on the seed layer.

[0021] In some embodiments, growing an epitaxial layer on the doped layer includes: in an environment of a second carrier gas, the second growth gas reacts to obtain the epitaxial layer grown on the doped layer.

[0022] In some embodiments, the growing of the doped layer on the seed layer further includes: introducing an oxygen source gas, wherein the concentration of the oxygen source gas is less than or equal to 1%; and / or, the growing of the epitaxial layer on the doped layer further includes: introducing a nitrogen source gas, wherein the concentration of the nitrogen source gas is less than or equal to 10%.

[0023] In some embodiments, the first growth gas and the second growth gas are the same; and / or, the first carrier gas and the second carrier gas are the same.

[0024] It can be understood that the beneficial effects that can be achieved by the method for preparing a single crystal diamond epitaxial wafer provided in the above embodiments of the present disclosure can refer to the beneficial effects of the single crystal diamond epitaxial wafer described above, and will not be repeated here.

[0025] On the other hand, a method for preparing a single crystal diamond substrate is provided, the method comprising: providing a single crystal diamond epitaxial wafer as described in any of the above embodiments; separating the epitaxial layer farthest from the seed crystal layer in the single crystal diamond epitaxial wafer from the doping layer to obtain a single crystal diamond substrate.

[0026] It can be understood that the beneficial effects that can be achieved by the method for preparing a single crystal diamond substrate provided in the above embodiments of the present disclosure can refer to the beneficial effects of the single crystal diamond epitaxial wafer mentioned above, and will not be repeated here. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions in the present disclosure, the following briefly introduces the drawings required to be used in some embodiments of the present disclosure. Obviously, the drawings described below are only drawings of some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can also be obtained based on these drawings. In addition, the drawings described below can be regarded as schematic diagrams, and are not limitations on the actual size of the product involved in the embodiments of the present disclosure, the actual process of the method, the actual timing of the signal, etc.

[0028] Figure 1 is a schematic structural diagram of a single crystal diamond epitaxial wafer according to some embodiments;

[0029] Figure 2 Based on Figure 1 Schematic diagram of the cross-sectional structure of a single crystal diamond epitaxial wafer along the AA section line;

[0030] Figure 3 is another schematic diagram of the structure of a single crystal diamond epitaxial wafer according to some embodiments;

[0031] Figure 4 is a flow chart of a method for preparing a single crystal diamond epitaxial wafer according to some embodiments;

[0032] Figure 5 1 is a structural diagram corresponding to each step of a method for preparing a single crystal diamond epitaxial wafer according to some embodiments. DETAILED DESCRIPTION

[0033] The following will be combined with the accompanying drawings to clearly and completely describe the technical solutions in some embodiments of the present disclosure. Obviously, the described embodiments are only part of the embodiments of the present disclosure, rather than all the embodiments. Based on the embodiments provided by the present disclosure, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present disclosure.

[0034] In the description of the present disclosure, it should be understood that the terms "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present disclosure and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present disclosure.

[0035] Unless the context requires otherwise, throughout the specification and claims, the term "including" is to be interpreted as an open, inclusive meaning, that is, "including, but not limited to". In the description of the specification, the terms "one embodiment", "some embodiments", "exemplary embodiments", "exemplarily" or "some examples" and the like are intended to indicate that specific features, structures, materials or characteristics associated with the embodiment or example are included in at least one embodiment or example of the present disclosure. The schematic representation of the above terms does not necessarily refer to the same embodiment or example. In addition, the specific features, structures, materials or characteristics may be included in any one or more embodiments or examples in any appropriate manner.

[0036] In the following, the terms "first" and "second" are used for descriptive purposes only and are not to be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the embodiments of the present disclosure, unless otherwise specified, "plurality" means two or more.

[0037] “At least one of A, B, and C” has the same meaning as “at least one of A, B, or C” and both include the following combinations of A, B, and C: A only, B only, C only, the combination of A and B, the combination of A and C, the combination of B and C, and the combination of A, B, and C.

[0038] “A and / or B” includes the following three combinations: A only, B only, and a combination of A and B.

[0039] In the context of the present disclosure, the meanings of “on,” “over,” and “over” should be interpreted in the broadest manner, so that “on” means not only “directly on something,” but also includes the meaning of “on something” with intervening features or layers therebetween, and “over” or “above” means not only “above” or “over” something, but also includes the meaning of “above” or “over” something without intervening features or layers therebetween (i.e., directly on something).

[0040] Exemplary embodiments are described herein with reference to cross-sectional views and / or plan views that are idealized exemplary drawings. In the drawings, the thickness of layers and regions are exaggerated for clarity. Therefore, variations in shape relative to the drawings due to, for example, manufacturing techniques and / or tolerances are conceivable. Therefore, the exemplary embodiments should not be interpreted as being limited to the shapes of the regions shown herein, but include shape deviations due to, for example, manufacturing. For example, an etched region shown as a rectangle will typically have curved features. Therefore, the regions shown in the drawings are schematic in nature, and their shapes are not intended to illustrate the actual shape of regions of the device, and are not intended to limit the scope of the exemplary embodiments.

[0041] Currently, Chemical Vapor Deposition (CVD) is a commonly used method for synthesizing diamond, among which Microwave Plasma Chemical Vapor Deposition (MPCVD) can be used to grow high-quality and large-area single-crystal diamond.

[0042] Microwave plasma chemical vapor deposition (MPCVD) mainly uses high-purity hydrogen (H 2 ) and methane (CH 4 ) and other reaction gases to form a high-power density plasma in a vacuum chamber, and use homoepitaxial growth on a diamond substrate to synthesize a diamond epitaxial layer of similar quality to the diamond substrate, and increase the area of ​​the synthesized diamond epitaxial layer and improve the synthetic thickness by adjusting the parameters and controlling the synthesis time. After the synthesis is completed, a laser or other material segmentation method is used to separate the diamond epitaxial layer from the diamond substrate to obtain a new single crystal diamond substrate. However, the single crystal diamond substrate prepared by the existing method has more impurities, greater surface roughness, and low yield, which limits the application and development of diamond.

[0043] Based on this, Figure 1 and Figure 2 As shown, an embodiment of the present disclosure provides a single crystal diamond epitaxial wafer 1000, which includes: a seed layer 101 and at least one group (i.e., one group or at least two groups) of stacked structures 20 grown on the seed layer 101. The stacked structure 20 includes: a doped layer 201 and an epitaxial layer 202 stacked along a first direction X, the material of the doped layer 201 is a single crystal diamond containing a first impurity, the first impurity is a substitutional impurity in the doped layer 201, and the material of the epitaxial layer 202 includes a single crystal diamond; wherein the first direction X is a direction perpendicular to the seed layer 101 and away from the seed layer 101.

[0044] It should be noted that the seed crystal is a small crystal with the same crystal orientation as the desired crystal, and is the seed for growing a single crystal, also called a seed crystal. For example, a single crystal diamond grown by a high temperature and high pressure method or a chemical vapor deposition method is used as the seed crystal layer 101, or a natural diamond is used as the seed crystal layer 101.

[0045] In some examples, such as Figure 1 and Figure 2 As shown, the single crystal diamond epitaxial wafer 1000 includes: a seed layer 101 and a group of stacked structures 20 grown on the seed layer 101 .

[0046] In some examples, such as Figure 3 As shown, the single crystal diamond epitaxial wafer 1000 includes: a seed layer 101 and two sets of stacked structures 20 grown on the seed layer 101 .

[0047] In some other examples, the single crystal diamond epitaxial wafer 1000 includes: a seed layer 101 and more than three stacked structures 20 grown on the seed layer 101 .

[0048] For example, Figure 2 As shown, the embodiment of the present disclosure uses a seed layer 101 and a doping layer 201 grown on the seed layer 101 as a substrate 100 for growing a single crystal diamond epitaxial layer 202. The epitaxial layer 202 is grown in this structural manner to improve the crystal quality of the epitaxial layer 202, for example, so that the epitaxial layer 202 has fewer impurities, less surface roughness, and higher consistency of crystal plane orientation. The single crystal diamond epitaxial wafer 1000 may include a plurality of stacked structures 20, which is related to a method for preparing a single crystal diamond epitaxial wafer 1000 for continuously improving the crystal quality of the epitaxial layer 202, and an epitaxial layer 202 with continuously improved crystal quality may be obtained. For an introduction to the method for preparing the single crystal diamond epitaxial wafer 1000, refer to the subsequent content, which will not be described in detail here.

[0049] It should be noted that the type of impurities in the crystal can be detected by Raman spectroscopy, and the content of impurities can be detected by the half-peak width of the Raman spectrum. Among them, Raman spectroscopy (Raman spectra) is a scattering spectrum, and the horizontal axis is the Raman shift, which is the wave number difference of the scattered light relative to the incident light (Raman shift cm -1 ), the vertical axis is the photon count, which is the intensity of scattered light. The half-peak width of the Raman spectrum refers to the peak width at half the peak height of the spectrum, that is, the distance between the two points where a straight line parallel to the bottom of the peak passes through the midpoint of the peak height and intersects the two sides of the peak.

[0050] The surface roughness is the arithmetic mean deviation of the crystal surface profile. The smaller the crystal surface roughness, the smoother the surface. Exemplarily, the surface roughness of the epitaxial layer 202 is detected by an atomic force microscope or a scanning electron microscope.

[0051] The consistency of the crystal plane orientation can be detected by XRD (X-ray diffraction) or scanning electron microscopy. XRD is a research method used to analyze the diffraction pattern of a material and obtain information such as the composition of the material, the structure or morphology of the atoms or molecules inside the material, etc.

[0052] Doping generally refers to the purposeful addition of a small amount of other elements or compounds into a material or matrix in order to improve the performance of a certain material or substance. In order to improve the quality of single crystal diamond, the embodiment of the present disclosure may dope impurities into the single crystal diamond to obtain a substrate 100 for growing an epitaxial layer 202 with improved crystal quality.

[0053] According to the distribution position of the impurities in the crystal, the impurities in the crystal are divided into two types, namely substitutional impurities and interstitial impurities. The atoms of interstitial impurities are located in the gaps between lattice atoms. The atoms of substitutional impurities replace lattice atoms and are located at lattice points. The first impurity is a substitutional impurity in the doping layer 201, and the atoms of the first impurity replace lattice atoms and are located at lattice points.

[0054] The embodiment of the present disclosure first grows a doping layer 201 on the seed layer 101, where the doping layer 201 is doped with a first impurity, and the first impurity is a substitutional impurity. The first impurity can exclude the content of other impurities that affect the crystal quality, thereby obtaining a doping layer 201 with improved quality, and then grows an epitaxial layer 202, which is conducive to the growth of a high-quality epitaxial layer 202.

[0055] In some examples, by doping the doping layer 201 with the first impurity, and the first impurity is a substitutional impurity, the surface roughness of the doping layer 201 can be lower than the surface roughness of the seed layer 101 .

[0056] In some examples, the impurity concentration of the doping layer 201 is lower than the impurity concentration of the seed layer 101 .

[0057] It should be noted that the impurity concentration refers to the number of atoms of the doped impurities per cubic centimeter. For example, the impurity concentration of the doping layer 201 refers to the number of atoms of the doped impurities per cubic centimeter of the doping layer 201.

[0058] Exemplarily, the impurities of the doping layer 201 include sulfur, and the impurities of the seed layer 101 include sulfur and silicon. The sulfur content of the doping layer 201 is lower than the sum of the sulfur and silicon contents in the seed layer 101 .

[0059] For example, the impurities in the seed layer 101 include Si impurities, and in the seed layer 101, substitutional Si impurities, interstitial Si impurities, or both may be included. In order to prevent the Si impurities in the doping layer 201 from affecting the quality of the doping layer 201, a first impurity that is a substitutional impurity exists in the doping layer 201, and the first impurity can exclude the Si impurities from being doped in the doping layer 201, so that the doping layer 201 with a lower impurity concentration can be formed, so that the quality of the doping layer 201 is improved.

[0060] Exemplarily, the Raman spectrum of the improved doping layer 201 has no impurity characteristic peaks, wherein the impurity characteristic peaks are characteristic peaks other than the diamond phase. For example, the impurity characteristic peaks include characteristic peaks of Si impurities and characteristic peaks of non-diamond phases, that is, the Raman spectrum of the doping layer 201 has no characteristic peaks of Si impurities and characteristic peaks of non-diamond phases, indicating that the crystal quality of the doping layer 201 is good.

[0061] For example, the Raman spectrum of the doped layer 201 has a peak at 1332.5 cm -1 The characteristic peak is the characteristic peak of single crystal diamond, and there is no peak at 1332.5cm -1 characteristic peaks other than the characteristic peaks of .

[0062] Since the quality of the epitaxially grown epitaxial layer 202 depends on the crystal quality of the substrate 100, that is, in the embodiment provided in the present disclosure, the quality of the epitaxial layer 202 depends on the quality of the doping layer 201 based on its growth, therefore, the crystal plane orientation consistency of the epitaxial layer 202 is equivalent to the crystal plane orientation consistency of the doping layer 201, and the surface roughness of the epitaxial layer 202 is equivalent to the surface roughness of the doping layer 201.

[0063] That is, the crystal plane orientation consistency of the epitaxial layer 202 detected by XRD or SEM is equivalent to the crystal plane orientation consistency of the doped layer 201. Equivalence here can be understood as the characterization results of the crystal plane orientation consistency of the epitaxial layer 202 and the crystal plane orientation consistency of the doped layer 201 detected by the same detection means are similar.

[0064] For example, the doped layer 201 and the epitaxial layer 202 have a high degree of consistency in crystal plane orientation, more than 80% of the surface area of ​​the doped layer 201 is composed of (100) crystal planes, the Euler angles {α, β, γ} represent the crystal plane orientation, and the difference between adjacent crystal plane orientations satisfies |Δα|≤5°, |Δβ|≤5°, |Δγ|≤5°. Moreover, more than 80% of the surface area of ​​the epitaxial layer 202 is composed of (100) crystal planes, and the difference between adjacent crystal plane orientations satisfies |Δα|≤5°, |Δβ|≤5°, |Δγ|≤5°.

[0065] The surface roughness of the epitaxial layer 202 detected by atomic force microscopy or scanning electron microscopy is equivalent to the surface roughness of the doped layer 201. That is, the surface roughness of the epitaxial layer 202 and the surface roughness of the doped layer 201 detected by the same detection means are similar.

[0066] Therefore, the embodiment of the present disclosure first grows a doped layer 201 with improved quality on the seed layer 101 and then grows an epitaxial layer 202 on the doped layer 201 with improved quality, which is beneficial for obtaining an epitaxial layer 202 with less impurities, less surface roughness and higher crystal orientation consistency.

[0067] In some examples, the first impurity includes sulfur. That is, the sulfur impurity is a substitutional impurity in the doping layer 201. The sulfur-doped doping layer 201 generates less non-diamond, and the sulfur impurity can exclude the Si impurity from being doped in the doping layer 201, so that the doping layer 201 with a lower impurity concentration can be formed, so that the quality of the doping layer 201 is improved.

[0068] In some other examples, the doping layer 201 is doped with sulfur and does not contain Si.

[0069] In some examples, the doping concentration of the first impurity ranges from 10 16 / cm 3 ~10 17 / cm 3 .

[0070] It should be noted that the doping concentration of the first impurity can be understood as the number of doped atoms of the first impurity.

[0071] For example, the concentration of sulfur doping ranges from 10 16 / cm 3 ~10 17 / cm 3 For example, the sulfur doping concentration is 10 16 / cm 3 , 2 x 10 16 / cm 3 4 x 10 16 / cm 3 5 x 10 16 / cm 3 7ⅹ10 16 / cm 3 8ⅹ10 16 / cm 3 9ⅹ10 16 / cm 3 or 10 17 Etc., there is no limitation here.

[0072] In some examples, such as Figure 2As shown, in a stacked structure 20 , the thickness d2 of the epitaxial layer 202 is greater than the thickness d1 of the doped layer 201 .

[0073] The design that the thickness d1 of the doped layer 201 is smaller than the thickness d2 of the epitaxial layer 202 can achieve the purpose of improving the crystal quality of the epitaxial layer 202, and can form an epitaxial layer 202 with less impurities, less surface roughness and high crystal orientation consistency.

[0074] In some examples, such as Figure 2 As shown, the thickness d1 of the doping layer 201 ranges from 200 μm to 1000 μm. For example, the thickness d1 of the doping layer 201 is 200 μm, 300 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm or 1000 μm, etc., which is not limited here.

[0075] In some examples, such as Figure 3 As shown, the single crystal diamond epitaxial wafer 1000 includes: at least two groups of stacked structures 20, in which the doped layer 201 is the first doped layer 21a, the epitaxial layer 202 is the first epitaxial layer 22a, the remaining doped layers 201 are the second doped layers 21b, and the remaining epitaxial layers 202 are the second epitaxial layers 22b.

[0076] Two or more stacked structures 20 are provided because during the preparation process of the single crystal diamond epitaxial wafer 1000, if the quality parameter of the grown epitaxial layer 202 does not meet the preset target, the stacked structure 20 formed by the epitaxial layer 202 that does not meet the preset quality parameter target and the doped layer 201 located on the side of the epitaxial layer 202 that does not meet the preset target close to the seed layer 101 is used as a part of the substrate 100, and the doped layer 201 and the epitaxial layer 202 are continued to grow. Among them, the epitaxial layer 202 that does not meet the preset quality parameter target is called the second epitaxial layer 22b, and the doped layer 201 located on the side of the epitaxial layer 202 that does not meet the preset quality parameter target close to the seed layer 101 is called the second doped layer 21b.

[0077] The stacked structure 20 formed by the epitaxial layer 202 and the doped layer 201 that do not meet the preset quality parameter target is used as part of the substrate 100, and the doped layer 201 and the epitaxial layer 202 are continued to grow, so that the crystal quality of the doped layer 201 and the epitaxial layer 202 can be continuously improved. The specific preparation method of the single crystal diamond epitaxial wafer 1000 and the introduction of the preset quality parameter target of the epitaxial layer 202 are described in the subsequent content, which will not be described in detail here.

[0078] Since the quality of the grown epitaxial layer 202 depends on the quality of the substrate 100 used, the doped layer 201 grown again is grown on the improved epitaxial layer 202, i.e. Figure 3As shown, the first doped layer 21a is grown on the second epitaxial layer 22b. Due to the setting of the second doped layer 21b, the crystal quality of the second epitaxial layer 22b is improved. The first doped layer 21a is grown on the second epitaxial layer 22b with improved crystal quality. The quality of the first doped layer 21a will be further improved. Therefore, the impurity concentration of the first doped layer 21a will be lower than the impurity concentration of the second doped layer 21b.

[0079] For example, the impurities of the first doping layer 21a include substitutional sulfur impurities, and the sulfur impurity content is very small. The Raman spectrum of the first doping layer 21a does not have characteristic peaks of sulfur impurities, nor does it have characteristic peaks of other impurities (such as Si) and non-diamond phase characteristic peaks. The presence of impurity characteristic peaks in the Raman spectrum of the second doping layer 21b makes the quality parameters of the second doping layer 21b fail to meet the preset target.

[0080] Exemplarily, the surface roughness of the first doping layer 21 a is lower than the surface roughness of the second doping layer 21 b , and the surface roughness of the first doping layer 21 a is further improved.

[0081] In a stacked structure 20, the crystal plane orientation consistency of the epitaxial layer 202 is equal to the crystal plane orientation consistency of the doped layer 201, and the surface roughness of the epitaxial layer 202 is equal to the surface roughness of the doped layer 201. The impurity concentration of the first doped layer 21a is lower than the impurity concentration of the second doped layer 21b, and the surface roughness of the first doped layer 21a is lower than the surface roughness of the second doped layer 21b. Therefore, the impurity concentration of the first epitaxial layer 22a is lower than the impurity concentration of the second epitaxial layer 22b, and the surface roughness of the first epitaxial layer 22a is lower than the surface roughness of the second epitaxial layer 22b.

[0082] Thus, a first epitaxial layer 22 a with improved quality parameters is obtained. The first epitaxial layer 22 a has less impurities, less surface roughness and high crystal orientation consistency.

[0083] It should be noted that in Figure 3 In the single crystal diamond epitaxial wafer 1000 shown, the thickness d11 of the first doped layer 21a and the thickness d12 of the second doped layer 21b may be the same or different, and there is no limitation here. The thickness d21 of the first epitaxial layer 22a and the thickness d22 of the second epitaxial layer 22b may be the same or different, and there is no limitation here.

[0084] It should be noted that in Figure 3 In the single crystal diamond epitaxial wafer 1000 shown, the sulfur doping concentration of the first doping layer 21 a and the sulfur doping concentration of the second doping layer 21 b may be the same or different, and there is no limitation thereto.

[0085] The embodiments of the present disclosure also provide a substrate 100 for growing a diamond epitaxial layer 202, the substrate 100 comprising: a seed layer 101 and at least one doping layer 201, wherein the at least one doping layer 201 is grown on one side of the seed layer 101, and the material of the doping layer 201 is single crystal diamond containing a first impurity, and the first impurity is a substitutional impurity in the doping layer 201.

[0086] Therefore, the embodiment of the present disclosure provides an application of a stacked doping layer 201 and a seed layer 101 as a substrate 100 for growing an epitaxial layer 202 .

[0087] In the embodiment of the present disclosure, a doped layer 201 is first grown on a seed layer 101 to form a substrate 100 for growing an epitaxial layer 202. Since the quality of the grown epitaxial layer 202 depends on the quality of the substrate 100 used therefor, an epitaxial layer 202 with better crystal quality can be obtained by growing a doped layer 201 with less impurities and less surface roughness on the seed layer 101 and using the seed layer 101 and the doped layer 201 as the substrate 100 to grow the epitaxial layer 202.

[0088] Therefore, the first impurity doped single crystal diamond can be used to form a doped layer 201 with less impurities and less surface roughness as an improvement layer for the growth of the epitaxial layer 202, and the seed layer 101 and the doped layer 201 form a substrate 100. The epitaxial layer 202 with good crystal quality is grown on the high-quality substrate 100, and the single crystal diamond substrate 30 with good quality (such as Figure 3 As shown in the figure, the problem that the high impurities in the grown epitaxial layer 202 in the prior art lead to low yield of the single crystal diamond substrate 30 is effectively solved. The introduction of cutting to obtain the single crystal diamond substrate 30 can refer to the introduction of the subsequent preparation method of the single crystal diamond substrate 30, which will not be described here.

[0089] In some examples, such as Figure 3 As shown, the number of doped layers 201 is at least two, and the substrate 100 for growing the diamond epitaxial layer 202 further includes: at least one epitaxial layer 202 , and the epitaxial layer 202 is located between two adjacent doped layers 201 .

[0090] Exemplarily, the number of the doped layers 201 is two, and an epitaxial layer 202 is disposed between the two doped layers 201 .

[0091] The diamond epitaxial layer 202 growth substrate 100 provided in the embodiment of the present disclosure will continue to grow the doped layer 201 on the epitaxial layer 202 that does not meet the preset quality parameter target, and can continuously improve the crystal quality of the doped layer 201 to provide a high-quality diamond epitaxial layer 202 growth substrate 100.

[0092] The embodiment of the present disclosure also provides a method for preparing a single crystal diamond epitaxial wafer 1000, such as Figure 4 As shown, the method includes: S1 to S3.

[0093] S1, such as Figure 5 As shown, a seed layer 101 is provided.

[0094] For example, a single crystal diamond grown by a high temperature and high pressure method or a chemical vapor deposition method uses a (100) oriented single crystal diamond as a seed layer 101, and the seed layer 101 can be used as a seed layer for growing single crystal diamond or doped single crystal diamond. For example, the length and width of the seed layer 101 are equal, the size is 10 mm x 10 mm, and the thickness of the seed layer 101 is 1000 μm.

[0095] The method for preparing the single crystal diamond epitaxial wafer 1000 further includes a step of pre-treating the seed layer 101, which includes: sequentially performing mechanical grinding and polishing, cleaning, surface drying, and plasma etching on the surface of the seed layer 101. The surface of the seed layer 101 is pre-treated to obtain a seed layer 101 with a surface roughness less than or equal to 1 nm.

[0096] The surface roughness of the seed layer 101 being less than or equal to 1 nm is beneficial to the growth of the high-quality doping layer 201 .

[0097] Exemplarily, the surface of the seed layer 101 is cleaned by using a sulfuric acid and nitric acid solution with a molar ratio of 1:1 at 300° C. to remove impurities generated during the polishing process, and then ultrasonic cleaning and secondary ultrasonic cleaning are performed using acetone, alcohol and deionized water.

[0098] The seed crystal layer 101 after mechanical surface grinding and polishing is pickled and cleaned in a preset strong acid. After the pickling and cleaning is completed, ultrasonic cleaning is performed in deionized water using ultrasound to remove pickling impurities so as to remove impurities generated during the pickling process. Then, a secondary ultrasonic cleaning is performed in acetone, alcohol and deionized water to remove solutes introduced during the pickling and ultrasonic cleaning processes for removing pickling impurities.

[0099] Exemplarily, the surface drying treatment of the seed crystal layer 101 includes: using dehumidified compressed air to blow dry the surface of the seed crystal layer 101 or drying the seed crystal layer 101 in a dust-free oven at 50° C. to 100° C.

[0100] Exemplarily, the surface of the seed layer 101 is subjected to plasma etching, including: placing the seed layer 101 in a microwave plasma chemical vapor deposition device for etching at a temperature of 800° C. to 900° C., etching for 10 minutes to 40 minutes under hydrogen and oxygen conditions, to remove surface impurities and defects remaining after polishing. For example, a microwave plasma chemical vapor deposition device with a specification of 2.45 GHz is used.

[0101] Finally, a seed layer 101 with a surface roughness less than or equal to 1 nm is obtained.

[0102] S2, such as Figure 5 As shown, a doping layer 201 is grown on the seed layer 101 ; the material of the doping layer 201 is single crystal diamond containing a first impurity, and the first impurity is a substitutional impurity in the doping layer 201 .

[0103] Exemplarily, the step of growing the doping layer 201 on the seed layer 101 includes: in an environment of a first carrier gas, reacting a first growth gas with a doping source gas to obtain the doping layer 201 grown on the seed layer 101 .

[0104] Specifically, the steps of preparing the doping layer 201 include: placing the seed crystal layer 101 after surface pretreatment in a microwave plasma chemical vapor deposition device, introducing a first growth gas, a doping source gas, an oxygen source gas and a first carrier gas after evacuation, and growing for 1 hour to 100 hours under the conditions of a power range of 1kW to 5.8kW, a pressure range of 5kPa to 25kPa and a temperature range of 600℃ to 1350℃ to obtain the doping layer 201.

[0105] For example, a microwave plasma chemical vapor deposition device with a specification of 2.45 GHz is used.

[0106] Exemplarily, the first growth gas includes at least one of methane, acetylene, acetone and ethanol. It is understandable that the first growth gas is a carbon source gas, and the carbon source gas grows into single crystal diamond on the seed layer 101 .

[0107] The concentration range of the first growth gas is 1% to 10%. The concentration of the first growth gas is the ratio of the volume of the first growth gas to the sum of the volumes of the first growth gas, the first carrier gas, the oxygen source gas, and the sulfur source gas. For example, the concentration of the first growth gas is 1%, 3%, 4%, 6%, 7%, 8%, 9%, or 10%, etc., and is not limited here. By setting the concentration range of the first growth gas to 1% to 10%, it is possible to avoid the generation of impurities due to insufficient ionization of the carbon source gas, which is conducive to the growth of single crystal diamonds with fewer impurities.

[0108] Exemplarily, the first carrier gas is hydrogen.

[0109] Exemplarily, the doping source gas includes a sulfur source gas, and the sulfur source gas includes at least one of sulfur dioxide and hydrogen sulfide. The formed doping layer 201 is a sulfur-doped single-crystal diamond. The sulfur source gas is introduced into the first growth gas, and the sulfur source gas is doped into the diamond lattice as a substitutional impurity during the growth of the single-crystal diamond, which can reduce impurities, improve the consistency of crystal plane orientation, and reduce surface roughness. Thus, a high-quality epitaxial layer 202 is obtained, achieving the effect of improving the quality of the epitaxial layer 202.

[0110] Exemplarily, the concentration of the sulfur source gas ranges from 10ppm to 100ppm. For example, the concentration of the sulfur source gas is 10ppm, 20ppm, 30ppm, 40ppm, 60ppm, 70ppm, 80ppm or 100ppm, etc., which is not limited here. Among them, ppm (parts per million) is a gas volume concentration of one millionth. Here, ppm means that the volume of the sulfur source gas accounts for one millionth of the sum of the volumes of the first growth gas, the first carrier gas, the oxygen source gas and the sulfur source gas.

[0111] When growing single crystal diamond, a sulfur source gas with a concentration range of 10ppm to 100ppm is added. The sulfur source gas content is relatively low, and a high-quality doping layer 201 with less impurities, higher crystal orientation consistency and less surface roughness can be obtained, thereby forming a high-quality substrate 100, which is beneficial to improving the crystal quality of the epitaxial layer 202.

[0112] Exemplarily, the oxygen source gas includes at least one of oxygen, carbon monoxide and carbon dioxide. When the oxygen source gas is introduced into the first growth gas, the oxygen atoms can be activated to etch the non-diamond phase in the diamond growth process, thereby improving the crystal quality. In addition, the addition of the oxygen source gas can prevent cracks from being generated when growing thicker single crystal diamonds, thereby achieving the purpose of preparing a high-quality doped layer 201, thereby obtaining a high-quality epitaxial layer 202, and achieving the effect of improving the quality of the epitaxial layer 202.

[0113] Exemplarily, the concentration of the oxygen source gas is less than or equal to 1%. The concentration of the oxygen source gas is the ratio of the volume of the oxygen source gas to the sum of the volumes of the first growth gas, the first carrier gas, the oxygen source gas, and the sulfur source gas. For example, the concentration of the oxygen source gas is 0.1%, 0.3%, 0.4%, 0.6%, 0.7%, 0.8% or 1%, etc., which is not limited here.

[0114] When growing single crystal diamond, adding sulfur source gas with a concentration range of 10ppm to 100ppm and oxygen source gas with a concentration less than or equal to 1% can obtain a high-quality doped layer 201 with less impurities, higher crystal orientation consistency and less surface roughness, thereby forming a high-quality epitaxial layer 202.

[0115] Exemplarily, the growth time of the doping layer 201 is 1 hour, 5 hours, 20 hours, 25 hours, 40 hours, 60 hours, 70 hours, 80 hours, 90 hours or 100 hours, etc., which is not limited here. By setting the growth time of the doping layer 201 to 1 hour to 100 hours, the doping layer 201 with a thickness d1 ranging from 200 μm to 1000 μm can be formed.

[0116] S3, such as Figure 5 As shown, an epitaxial layer 202 is grown on the doped layer 201; the material of the epitaxial layer 202 includes single crystal diamond.

[0117] In some examples, growing the epitaxial layer 202 on the doping layer 201 includes: in an environment of a second carrier gas, a second growth gas reacts to obtain the epitaxial layer 202 grown on the doping layer 201 .

[0118] Specifically, preparing the epitaxial layer 202 includes: introducing a nitrogen source gas, a second growth gas and a second carrier gas in a microwave plasma chemical vapor deposition device, growing the epitaxial layer 202 on the substrate 100 under conditions of a power range of 1 kW to 5.8 kW, a pressure range of 5 kPa to 25 kPa and a temperature range of 600°C to 1350°C, for a time range of 1 hour to 1000 hours and a growth rate of 1 μm / hour to 30 μm / hour.

[0119] Exemplarily, the second growth gas includes at least one of methane, acetylene, acetone and ethanol. It is understandable that the second growth gas is a carbon source gas, and the carbon source gas grows on the doping layer 201 to form a single crystal diamond.

[0120] The concentration range of the second growth gas is 1% to 10%. The concentration of the second growth gas is the ratio of the volume of the second growth gas to the sum of the volumes of the second growth gas, the second carrier gas and the nitrogen source gas. For example, the concentration of the second growth gas is 1%, 3%, 4%, 6%, 7%, 8%, 9% or 10%, etc., and is not limited here. By setting the concentration range of the second growth gas to 1% to 10%, it is possible to avoid the generation of impurities due to insufficient ionization of the carbon source gas, which is conducive to the growth of single crystal diamonds with fewer impurities.

[0121] In some examples, the first growth gas and the second growth gas are the same. After the growth of the doping layer 201 is completed, the epitaxial layer 202 is grown under the same growth gas, which can make the process implementation easier.

[0122] In some examples, the first carrier gas and the second carrier gas are the same, both of which are hydrogen. After the growth of the doping layer 201 is completed, the epitaxial layer 202 is grown under the same carrier gas, which can make the process implementation easier.

[0123] That is, based on step S2, the concentrations of the doping source gas and the oxygen source gas in the microwave plasma chemical vapor deposition equipment are adjusted to zero, and the nitrogen source gas is turned on. The growth of the doping layer 201 and the growth of the epitaxial layer 202 use the same growth gas and carrier gas.

[0124] The introduction of nitrogen source gas can increase the growth rate of the epitaxial layer 202 .

[0125] For example, the nitrogen source gas includes: at least one of nitrogen and ammonia. The concentration of the nitrogen source gas is less than or equal to 10%, wherein the concentration of the nitrogen source gas is the ratio of the volume of the nitrogen source gas to the sum of the volumes of the second growth gas, the second carrier gas and the nitrogen source gas. For example, the concentration of the nitrogen source gas is 1%, 3%, 4%, 6%, 7%, 8%, 9% or 10%, etc., and is not limited here. By setting the concentration of the nitrogen source gas to be less than or equal to 10%, the growth rate of the epitaxial layer 202 can be effectively increased.

[0126] Exemplarily, the time taken to grow the epitaxial layer 202 is 1 hour, 50 hours, 100 hours, 200 hours, 300 hours, 450 hours, 500 hours, 700 hours or 1000 hours, etc., which is not limited here. By setting the time taken to grow the epitaxial layer 202 to 1 hour to 1000 hours, an epitaxial layer 202 with a thickness d2 in the range of 500 μm to 5000 μm can be formed, thereby obtaining a single crystal diamond substrate 30 with a thickness in the range of 500 μm to 5000 μm, wherein the single crystal diamond substrate 30 with a thickness in the range of 500 μm to 5000 μm is a single crystal diamond substrate 30 that meets the thickness requirement.

[0127] Exemplarily, the growth rate of the epitaxial layer 202 is 1 μm / hour, 3 μm / hour, 6 μm / hour, 12 μm / hour, 19 μm / hour, 20 μm / hour, 25 μm / hour or 30 μm / hour, etc., which is not limited here. By controlling the growth rate of the epitaxial layer 202 to be 1 μm / hour to 30 μm / hour, it is beneficial to control the formation of a high-quality epitaxial layer 202.

[0128] Exemplarily, when the thickness d2 of the epitaxial layer 202 reaches a required value, the growth is terminated.

[0129] Since the quality of the grown epitaxial layer 202 depends on the quality of the doping layer 201 on which it is grown, the epitaxial layer 202 grown on the doping layer 201 with fewer impurities, higher crystal orientation consistency and smaller surface roughness also has higher crystal quality, thereby achieving the purpose of improving the crystal quality of the epitaxial layer 202 by setting the doping layer 201.

[0130] In some embodiments, the method for preparing the single crystal diamond epitaxial wafer 1000 further includes: if the quality parameters of the epitaxial layer 202 do not meet the preset targets, returning to the step of growing the doped layer 201 and the step of growing the epitaxial layer 202 until the quality parameters of the epitaxial layer 202 meet the preset targets; the quality parameters of the epitaxial layer 202 include at least one of impurities and surface roughness.

[0131] Exemplarily, the deposits on the surface of the single crystal diamond epitaxial wafer 1000 are removed, and then the impurities and surface roughness of the epitaxial layer 202 are detected. For example, the deposits include non-diamond phase impurities such as graphite carbon.

[0132] Exemplarily, when the quality parameters of the epitaxial layer 202 include impurities, the preset targets include: the Raman spectrum of the epitaxial layer 202 has no impurity characteristic peaks, and the impurity characteristic peaks are characteristic peaks outside the diamond phase. When the quality parameters of the epitaxial layer 202 include surface roughness, the preset targets include: the surface roughness of the epitaxial layer 202 is less than the surface roughness of the seed layer 101. When the impurities and surface roughness of the epitaxial layer 202 do not meet the preset targets, the doping layer 201 is continued to be grown in the microwave plasma chemical vapor deposition equipment, the second quality improvement step is performed, and the epitaxial layer 202 is grown again, and the quality of the epitaxial layer 202 grown again will be improved to a certain extent relative to the quality of the epitaxial layer 202 grown the previous time. This is more conducive to the growth of an epitaxial layer 202 with fewer impurities, smaller surface roughness, and higher consistency of crystal orientation.

[0133] For example, the impurities of the epitaxial layer 202 are detected by Raman spectroscopy, the crystal orientation consistency of the epitaxial layer 202 is detected by XRD or scanning electron microscopy, and the surface roughness of the epitaxial layer 202 is observed by scanning electron microscopy.

[0134] Furthermore, the performance of the epitaxial layer 202 can be characterized by the half-peak width of the Raman spectrum. The half-peak width of the Raman spectrum represents the grain size of the crystal. The smaller the grain, the more severe the broadening; conversely, the larger the grain, the sharper the diffraction peak. It should be noted that the half-peak width ranges from 1.6 cm -1 ~4.5cm -1 , it means that the grain size of the epitaxial layer 202 meets the requirements. The half-peak width of the epitaxial layer 202 provided in the embodiment of the present disclosure is 2.0 cm -1 , indicating that the grain size of the epitaxial layer 202 provided in the embodiment of the present disclosure meets the requirements.

[0135] In addition, in the PL spectrum (Photoluminescence Spectroscopy) of the epitaxial layer 202, there are no characteristic peaks of other impurities, for example, no characteristic peaks of Si impurities, which indicates that the impurity quality parameters of the epitaxial layer 202 provided by the embodiment of the present disclosure meet the requirements.

[0136] By observing the surface of the epitaxial layer 202 through a scanning electron microscope, it can be seen that the surface of the epitaxial layer 202 is relatively smooth, which means that the surface roughness of the epitaxial layer 202 is relatively small and the crystal quality is relatively high.

[0137] The epitaxial layer 202 that does not meet the preset quality parameter target, and the doped layer 201 located on the side of the epitaxial layer 202 that does not meet the preset quality parameter target close to the seed layer 101 are a group of stacked structures 20. The epitaxial layer 202 that does not meet the preset quality parameter target is called the second epitaxial layer 22b, and the doped layer 201 located on the side of the epitaxial layer 202 that does not meet the preset quality parameter target close to the seed layer 101 is called the second doped layer 21b. The preparation method of the single crystal diamond epitaxial wafer 1000 provided in the embodiment of the present disclosure does not require an additional removal process to remove the epitaxial layer 202 and the doped layer 201 that do not meet the preset quality parameter target, which can reduce the loss of the substrate 100 material during the manufacturing process, reduce the risk of fragmentation, and extend the service life of the substrate 100.

[0138] In some embodiments, the method for preparing the single crystal diamond epitaxial wafer 1000 further includes: if the epitaxial layer 202 does not meet the thickness parameter target, returning to the step of growing the epitaxial layer 202 until the epitaxial layer 202 meets the thickness parameter target.

[0139] Exemplarily, the target thickness parameter of the epitaxial layer 202 includes: the thickness d2 of the epitaxial layer 202 is in the range of 500 μm to 5000 μm.

[0140] For example, the thickness d2 of the epitaxial layer 202 can be measured with a micrometer. The thickness d2 of the epitaxial layer 202 is 500 μm, 1000 μm, 1500 μm, 2000 μm, 3000 μm, 4500 μm or 500 μm, which is not limited here.

[0141] Therefore, the embodiment of the present disclosure continuously improves the quality of the doped layer 201 and thus continuously improves the quality of the epitaxially grown epitaxial layer 202, thereby obtaining a high-quality epitaxial layer 202, which not only improves the yield of the single crystal diamond epitaxial wafer 1000, but also effectively reduces the manufacturing cost.

[0142] The embodiment of the present disclosure also provides a method for preparing a single crystal diamond substrate 30, the method comprising: providing a single crystal diamond epitaxial wafer 1000 as provided in any of the above embodiments, and separating the epitaxial layer 202 farthest from the seed layer 101 in the single crystal diamond epitaxial wafer 1000 from the doping layer 201 to obtain the single crystal diamond substrate 30.

[0143] For example, Figure 3 As shown, a laser cutting method is adopted, using a pulsed laser operating at 532nm or 1064nm, and the epitaxial layer 202 is cut from the substrate 100 through an electrically controlled machine tool, and the cut epitaxial layer 202 is formed into a single crystal diamond substrate 30.

[0144] Therefore, the doping layer 201 used in the embodiment of the present disclosure is doped with substitutional impurities, forming a doping layer 201 with less impurities and less surface roughness as an improvement layer for the growth of the epitaxial layer 202. The epitaxial layer 202 with better crystal quality can be grown, and a single crystal diamond substrate 30 with better quality is obtained by cutting, which effectively solves the problem of high impurities in the grown epitaxial layer 202 in the prior art, resulting in a low yield of the single crystal diamond substrate 30.

[0145] Furthermore, the epitaxial layer 202 can be grown again on the substrate 100 to prepare a new single crystal diamond substrate 30, that is, the substrate 100 can be used again to achieve the purpose of recycling.

[0146] Therefore, the embodiments of the present disclosure provide a single crystal diamond epitaxial wafer 1000 that can prepare high-quality single crystal diamond substrates 30, and a method for preparing single crystal diamond epitaxial wafer 1000 that continuously improves the quality of single crystal diamond epitaxial layer 202, so as to solve the problem of low yield of diamond substrates 30 caused by high impurities, poor crystal plane orientation consistency and high surface roughness of single crystal diamond prepared in the prior art.

[0147] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A single crystal diamond epitaxial wafer, characterized in that: include: seed layer; A stacked structure grown on the seed crystal layer, the stacked structure comprising: a doped layer and an epitaxial layer stacked along a first direction, the material of the doped layer is a single crystal diamond containing a first impurity, the first impurity is a substitutional impurity in the doped layer, the first impurity can exclude the content of other impurities that affect the quality of the crystal, and the doping concentration range of the first impurity is 10 16 / cm 3 ~10 17 / cm 3 , the material of the epitaxial layer includes single crystal diamond; wherein the first direction is a direction perpendicular to the seed crystal layer and away from the seed crystal layer; In the stacked structure farthest from the seed layer, the doped layer is a first doped layer, the doped layer close to the seed layer is a second doped layer, and the impurity concentration of the first doped layer is lower than the impurity concentration of the second doped layer.

2. The single crystal diamond epitaxial wafer according to claim 1, characterized in that: The surface roughness of the doping layer is lower than the surface roughness of the seed layer; and / or, The impurity concentration of the doping layer is lower than the impurity concentration of the seed layer.

3. The single crystal diamond epitaxial wafer according to claim 1, characterized in that: The consistency of the crystal plane orientation of the epitaxial layer is equal to the consistency of the crystal plane orientation of the doped layer; and / or, The surface roughness of the epitaxial layer is equal to the surface roughness of the doped layer.

4. The single crystal diamond epitaxial wafer according to claim 1, characterized in that: The first impurity includes sulfur.

5. The single crystal diamond epitaxial wafer according to claim 1, characterized in that: In a group of the stacked structures, the thickness of the epitaxial layer is greater than the thickness of the doped layer.

6. The single crystal diamond epitaxial wafer according to any one of claims 1 to 5, characterized in that: In the stacked structure farthest from the seed crystal layer, the epitaxial layer is the first epitaxial layer, and the remaining epitaxial layers are the second epitaxial layers; The surface roughness of the first doped layer is lower than the surface roughness of the second doped layer; and / or, The impurity concentration of the first epitaxial layer is lower than the impurity concentration of the second epitaxial layer; and / or, The surface roughness of the first epitaxial layer is lower than the surface roughness of the second epitaxial layer.

7. A substrate for growing a diamond epitaxial layer, characterized in that: include: seed layer; A doping layer is grown on one side of the seed crystal layer; the material of the doping layer is a single crystal diamond containing a first impurity, the first impurity is a substitutional impurity in the doping layer, the first impurity can exclude the content of other impurities that affect the quality of the crystal, and the doping concentration range of the first impurity is 10 16 / cm 3 ~10 17 / cm 3 ; The doping layer farthest from the seed layer is a first doping layer, and the doping layer close to the seed layer is a second doping layer. The impurity concentration of the first doping layer is lower than the impurity concentration of the second doping layer.

8. The diamond epitaxial layer growth substrate according to claim 7, characterized in that: The surface roughness of the doping layer is lower than the surface roughness of the seed layer; and / or, The impurity concentration of the doping layer is lower than the impurity concentration of the seed layer.

9. The substrate for growing a diamond epitaxial layer according to claim 7 or 8, characterized in that: Also includes: At least one epitaxial layer, wherein the epitaxial layer is located between two adjacent doped layers.

10. A method for preparing a single crystal diamond epitaxial wafer, characterized in that: include: providing a seed layer; A doping layer is grown on the seed layer; the material of the doping layer is a single crystal diamond containing a first impurity, the first impurity is a substitutional impurity in the doping layer, the first impurity can exclude the content of other impurities that affect the quality of the crystal, and the doping concentration range of the first impurity is 10 16 / cm 3 ~10 17 / cm 3 ; growing an epitaxial layer on the doped layer; the material of the epitaxial layer comprises single crystal diamond; If the quality parameters of the epitaxial layer do not meet the preset targets, return to the step of growing the doped layer and the step of growing the epitaxial layer until the quality parameters of the epitaxial layer meet the preset targets; the quality parameters of the epitaxial layer include at least one of impurities and surface roughness; wherein the doped layer farthest from the seed layer is the first doped layer, and the doped layer close to the seed layer is the second doped layer, and the impurity concentration of the first doped layer is lower than the impurity concentration of the second doped layer.

11. The method for preparing a single crystal diamond epitaxial wafer according to claim 10, characterized in that: Also includes: If the epitaxial layer does not meet the thickness parameter target, the step of growing the epitaxial layer is returned to be executed until the epitaxial layer meets the thickness parameter target.

12. The method for preparing a single crystal diamond epitaxial wafer according to claim 11, characterized in that: When the quality parameter of the epitaxial layer includes impurities, the preset target includes: the Raman spectrum of the epitaxial layer has no impurity characteristic peak, and the impurity characteristic peak is a characteristic peak other than the diamond phase; When the quality parameter of the epitaxial layer includes surface roughness, the preset target includes: the surface roughness of the epitaxial layer is less than the surface roughness of the seed crystal layer; The thickness parameter target of the epitaxial layer includes: the thickness range of the epitaxial layer is 500 μm to 5000 μm.

13. The method for preparing a single crystal diamond epitaxial wafer according to any one of claims 10 to 12, characterized in that: The step of growing a doped layer on the seed layer comprises: In an environment of a first carrier gas, a first growth gas is reacted with a doping source gas to obtain a doping layer grown on the seed crystal layer.

14. The method for preparing a single crystal diamond epitaxial wafer according to claim 13, characterized in that: The step of growing an epitaxial layer on the doped layer comprises: In an environment of the second carrier gas, the second growth gas reacts to obtain an epitaxial layer grown on the doped layer.

15. The method for preparing a single crystal diamond epitaxial wafer according to claim 14, characterized in that: The step of growing a doped layer on the seed layer further includes: introducing an oxygen source gas, wherein the concentration of the oxygen source gas is less than or equal to 1%; and / or, The method of growing an epitaxial layer on the doped layer further comprises: introducing a nitrogen source gas, wherein the concentration of the nitrogen source gas is less than or equal to 10%.

16. The method for preparing a single crystal diamond epitaxial wafer according to claim 14 or 15, characterized in that: The first growth gas and the second growth gas are the same; and / or, The first carrier gas and the second carrier gas are the same.

17. A method for preparing a single crystal diamond substrate, characterized in that: include: Providing a single crystal diamond epitaxial wafer as claimed in any one of claims 1 to 6; The epitaxial layer farthest from the seed crystal layer in the single crystal diamond epitaxial wafer is separated from the doped layer to obtain a single crystal diamond substrate.