A continuous extrusion-molded ultra-high performance cement-based tile and its preparation process

By combining ultra-high performance concrete and extrusion forming process, cellulose ether, composite modified components and modified machine sand are used to solve the problem of insufficient strength and area of ​​traditional cement base tiles, and high-efficiency production is achieved. Durable cement tiles are suitable for industrial buildings and extend the service life of roof structures.

CN117550844BActive Publication Date: 2024-11-19HUAXIN CEMENT CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311854737.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-11-19
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

Traditional cement base tiles have low strength, small area and low production efficiency, and cannot replace color steel tiles in the industrial field, and ultra-high performance concrete is difficult to extrude.

Method used

Ultra-high performance concrete and extrusion molding process are combined, and high-strength is prepared by adding cellulose ether, composite modified components, compensating shrinkage components and modified machine sand, combined with vacuum spiral extruder and steam maintenance process. , high durability and large single-piece cement tiles.

Benefits of technology

Ultra-high performance cement tiles with efficient continuous extrusion are achieved, which improves mechanical properties and durability. They are suitable for industrial construction fields, extend the service life of roof structures, and improve production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004641910710000061
    Figure BDA0004641910710000061
  • Figure BDA0004641910710000071
    Figure BDA0004641910710000071
  • Figure HDA0004641910720000011
    Figure HDA0004641910720000011
Patent Text Reader

Abstract

The present invention discloses a continuous extrusion-molded ultra-high performance cement-based tile, which uses cement, silica fume, mineral powder, fly ash microbeads, modified machine-made sand, steel fiber, composite modified component, water reducer, shrinkage compensating component, cellulose ether, and water as main raw materials; the composite modified component includes nano magnesium aluminum silicate, graphite powder, and polymer water-absorbing resin; the modified machine-made sand is machine-made sand after ball milling, screening, and hydrophobic modification. The present invention applies the ultra-high performance concrete formula system to the preparation of ultra-cement-based tiles, and combines the modification means such as cellulose ether, modified machine-made sand, composite modified component, shrinkage compensating component, etc., to effectively improve the mechanical properties and durability of the obtained cement-based tiles under the premise of ensuring the continuous extrusion molding effect, and is conducive to improving production efficiency, which can provide a new idea for the preparation of high-performance and large-size cement-based tiles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and in particular relates to a continuously extruded ultra-high performance cement-based tile and a preparation process thereof. Background Art

[0002] Traditional cement-based tiles are usually produced by filter pressing, molding or extrusion, but there are various problems, such as: the material type is single (basically cement, sand, water, glass fiber), resulting in poor mechanical properties and durability of the tiles; traditional fiber cement-based tiles, asbestos tiles, etc. have been gradually replaced by color steel tiles due to their general bearing capacity and durability. At the same time, cement tiles produced by traditional molding and extrusion methods are limited by materials and equipment, and the tiles produced are small tiles, mainly used for roof decoration, thermal insulation, etc. of civil buildings. They cannot be used on a large scale in industrial plants and other fields, let alone replace color steel tiles. Compared with the color steel tiles and resin tiles commonly used in factories, cement tiles have good anti-corrosion and weather resistance. If new cement tiles with high bearing capacity, excellent durability and large single-piece area can be produced, they can perfectly replace the existing color steel tiles and increase the service life of the roof structure.

[0003] Ultra-high performance concrete is a new type of building material that does not contain coarse aggregate and is mixed with steel fiber. If ultra-high performance concrete materials can be combined with extrusion molding technology, material modification optimization and process matching design can be carried out for the production of extrusion-molded cement-based tiles, it will have huge market potential. However, ultra-high performance concrete is a large fluid material and is usually not suitable for extrusion molding. Therefore, the key issues that need to be solved in the preparation of continuously extruded ultra-high performance cement-based tiles include achieving smooth extrusion of tile products while ensuring ultra-high strength, durability, and preparation efficiency. Summary of the invention

[0004] The main purpose of the present invention is to provide a continuously extruded ultra-high performance cement-based tile to solve the problems of low strength, small area, low production efficiency and inability to replace color steel tiles for large-scale application in the industrial field.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A continuously extruded ultra-high performance cement-based tile, the raw materials required and their weight proportions include: 650-800 parts of cement, 160-200 parts of silica fume, 100-130 parts of mineral powder, 60-100 parts of fly ash microbeads, 1000 parts of modified machine-made sand, 120-150 parts of steel fiber, 4-9 parts of composite modified components, 3-6 parts of water reducer, 20-30 parts of shrinkage compensating components, 2-6 parts of cellulose ether, and 180-230 parts of water; the composite modified components include nano magnesium aluminum silicate, graphite powder and high molecular water-absorbing resin; the modified machine-made sand is machine-made sand after ball milling, screening and hydrophobic modification.

[0007] In the above scheme, the mass ratio of the nano magnesium aluminum silicate, graphite powder and polymer water-absorbing resin is 1:0.3-0.7:0.3-0.8.

[0008] Furthermore, the purity of the nano magnesium aluminum silicate is above 90%, and the particle size is 10-50nm; the particle size of the graphite powder is 10-20μm; the particle size of the polymer water-absorbing resin is 40-80μm, and the water absorption multiple is 100-400 times.

[0009] In the above scheme, the hydrophobic modification step uses a silane coupling agent solution to soak the machine-made sand (18-24 hours). In the above scheme, the concentration of the silane coupling agent solution is 8-12wt%.

[0010] In the above scheme, the silane coupling agent can be selected from one or more of isooctyltriethoxysilane coupling agent, methyltrimethoxysilane and the like.

[0011] In the above scheme, the modified machine-made sand ball milling process is: the original machine-made sand is screened to remove aggregates with a particle size below 70 mesh, and the ball milling is performed at a ball milling rate of 50-70r / min for 40-80s.

[0012] In the above scheme, the screening step is to screen out granules with a particle size of 20-70 mesh.

[0013] In the above scheme, the components in the shrinkage compensating component and their weight proportions include: 8-12 parts of sulphoaluminate clinker and 4-5 parts of magnesium oxide.

[0014] In the above scheme, the cement is silicate cement, and specifically PII 52.5 or PO 52.5 silicate cement can be selected.

[0015] In the above scheme, the SiO2 content of the silica fume is ≥96%, and the 28d activity index is ≥110%.

[0016] In the above scheme, the 28d activity index of the mineral powder is ≥105%.

[0017] In the above scheme, the water demand ratio of the fly ash microspheres is ≤95%, the 28d activity index is ≥96%, and the glass content is ≥90%.

[0018] In the above solution, the steel fiber has a length of 5-6 mm and a diameter of 0.1-0.12 mm.

[0019] In the above scheme, the water reducing agent is a polycarboxylic acid high-efficiency water reducing agent, and its water reducing rate is 25-30%.

[0020] In the above scheme, the cellulose ether is hydroxyethyl cellulose ether.

[0021] The above-mentioned preparation process of the ultra-high performance cement-based tile formed by continuous extrusion comprises the following steps:

[0022] 1) Mixing: adding the modified component to part of the water to obtain a mixture A, dry-mixing the other raw materials except water, adding the remaining amount of water and the mixture A, stirring, and obtaining a blank;

[0023] 2) Extrusion: Use a vacuum screw extruder to extrude the obtained blank into a tile mold and cut it;

[0024] 3) Curing: The obtained green tile with the tile mold is subjected to steam curing and demoulding to obtain the ultra-high performance cement-based tile.

[0025] In the above scheme, in step 1), water accounting for 30-40% of the total amount is first added.

[0026] In the above scheme, the dry mixing time is 3-5 minutes.

[0027] In the above scheme, the stirring treatment time is 10-20 minutes.

[0028] In the above scheme, the extrusion process adopts vacuum twin-screw extrusion, the extrusion pressure is 3-6MPa, the vacuum degree is 10 -2 -10 -5 Pa, extrusion rate is 500-1000mm / min.

[0029] Furthermore, the steam curing temperature is 60-90°C and the time is 36-60h.

[0030] Furthermore, the ultra-high performance cement-based tiles are colored according to usage requirements.

[0031] In the above scheme, in the cutting step: the tile mold running speed is consistent with the extrusion speed of the blank, when the infrared sensing device (7) arranged on the cutting machine (6) senses the front end of the tile mold, the synchronous cutting machine (6) is started to cut the tile blank, the cutting machine is consistent with the tile mold speed along the conveyor belt direction, and at the same time, it cuts at a uniform speed perpendicular to the conveyor belt direction (along the width direction of the tile mold), after cutting, the cutting machine moves in the opposite direction along the conveyor belt and resets to the opposite side of the original position (along the width direction of the tile mold); reciprocating cutting is performed in this way. The above cutting step can effectively ensure the cutting quality of cement tile products on the basis of ensuring continuous extrusion processing.

[0032] The technical principle adopted by the present invention is:

[0033] 1) The present invention utilizes the characteristics of high durability and high strength of ultra-high performance concrete, and applies it to the preparation of cement-based tiles to give full play to the high strength and high toughness of the material, broaden the application scenarios of ultra-high performance concrete, and effectively improve the bearing capacity and durability of cement-based tiles. However, ultra-high performance concrete is a large fluid material and cannot be extruded and shaped. In order to solve the above technical problems, the present invention first adds cellulose ether, which can effectively increase the viscosity of the slurry and make it have a certain plasticity, but due to the increase in viscosity and the thin thickness of the tile extrusion port, it cannot be extruded smoothly; further introduces a composite modified component, in which the water-absorbing resin is pre-absorbed during the mixing process. On the basis of ensuring the working performance of the mixture, the extrusion pressure and vacuum environment can be used during the billet extrusion process to promote the water-absorbing resin to release part of the free water, and form a water film between the surfaces of cement and other particles, which has a good lubricating effect on the particles. At the same time, combined with graphite powder, the friction resistance between cement, silica fume and other particles in the extrusion process is further reduced, and the resulting billet is smoothly extruded from the corrugated extrusion port through the synergistic effect of the two. In addition, since the prepared tiles are cement-based ultra-thin structures, they are very likely to deform after being put into molds using conventional means. The present invention further introduces nano-magnesium aluminum silicate, whose three-dimensional network structure can provide skeleton support at the nano-micrometer level, further ensuring the thickness uniformity and square size of the tiles, and preventing deformation, mold collapse and other undesirable defects.

[0034] 2) In terms of aggregate, in order to reduce the material cost of cement-based tiles, machine-made sand is introduced as aggregate. However, as artificially crushed sand, the surface of machine-made sand is mostly angular and rough, which increases the friction coefficient between aggregate and cement particles. In order to reduce friction resistance, the machine-made sand is pre-treated by ball milling to reduce the roughness of the surface of the machine-made sand. At the same time, it is soaked with a silane coupling agent to form a hydrophobic film on its surface. This method can effectively improve the lubrication effect between machine-made sand and cement and other particles, and reduce the water absorption rate of the machine-made sand itself, further ensuring that the resulting mixture is smoothly extruded at the thin extrusion port.

[0035] 3) Since conventional ultra-high performance concrete uses a large amount of cementitious materials, and the cement tiles prepared by the present invention are ultra-thin structures, they are prone to shrinkage cracking and other problems. The compensating shrinkage component can play a compensating shrinkage role at different times in the early and later stages, reducing the risk of tile cracking.

[0036] 4) In terms of technology, the present invention abandons the conventional extrusion process idea, and makes the tile mold and the extruded tile run synchronously, and the cutting device has a horizontal and vertical synchronous operation mechanism, so that the tiles of the production line can be cut synchronously and with high quality without stopping operation.

[0037] The present invention introduces the design concept of ultra-high performance concrete materials. Compared with traditional cement-based tiles, high-activity cementitious materials such as cement, silica fume, and mineral powder can greatly improve the matrix strength under low water consumption, and can use the extrusion method to continuously produce cement-based tiles with a thickness of 5-7mm and a width of 800-1000mm; at the same time, it can effectively improve the toughness of the tiles, and the maximum length of the obtained ultra-high performance cement-based tiles can reach 5m.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] 1) The present invention proposes for the first time to apply ultra-high performance concrete to the preparation of ultra-cement-based tiles, and combines modification methods such as cellulose ether, modified machine-made sand, composite modified components, and shrinkage compensation components to achieve efficient and continuous extrusion molding of ultra-high performance concrete, which can provide a new idea for the preparation of high-performance cement-based tiles and effectively broaden the application field of ultra-high performance concrete;

[0040] 2) Under the premise of ensuring the continuous extrusion molding effect, the present invention can effectively improve the mechanical properties and durability of the obtained cement-based tiles, and is conducive to the efficient preparation of cement-based tiles with a larger single area; it can widely replace existing color steel tiles, resin tiles and other products in the field of industrial construction and civil use, and effectively improve the service life of the roof structure;

[0041] 3) The preparation method of the present invention is relatively simple, and can effectively improve the production efficiency of cement-based tiles, and is suitable for popularization and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 A schematic diagram of the structure of the extrusion equipment used in the present invention;

[0043] In the figure, 1 is an extrusion type conical hopper, 2 is a vacuum screw extruder, 3 is a corrugated extrusion port, 4 is a transition conveying device, 5 is a tile die, 6 is a cutting machine, and 7 is an infrared sensing device.

[0044] Figure 2 This is a physical picture of the ultra-high performance cement-based tile obtained in the example. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0046] In the following examples, the cement used is PII 52.5 cement; the silica fume SiO2 content is 96%, and the 28d activity index is 110%; the mineral powder is S105 grade, and the 28d activity index is 110%; the water requirement ratio of fly ash microspheres is 93%, the 28d activity index is 98%, and the glass content is 92%. The steel fiber length is 5-6mm and the diameter is 0.1-0.12mm; the water reducer is a polycarboxylic acid high-efficiency water reducer, and its water reduction rate is 26%; the cellulose ether is hydroxyethyl cellulose ether;

[0047] The preparation method of the modified machine-made sand is as follows: the original machine-made sand is screened to remove aggregates with a particle size below 70 mesh, and the sieve is placed in a ball mill with a ball milling rate of 60r / min and a time of 60s, and then the particle size of 20-70 mesh is screened out, and then it is placed in a 10wt% concentration of isooctyltriethoxysilane coupling agent and immersed for 24h, and then dried at 60°C to obtain the modified machine-made sand; wherein, the original machine-made sand is provided by the Huaxin Cement 100 million ton line machine-made sand project, and its parent rock is limestone, with a fineness modulus of 2.5 and a crushing value of 10%.

[0048] The shrinkage compensating component is composed of 10 parts of sulphoaluminate clinker and 4 parts of magnesium oxide; the composite modification component is composed of 1 part of high-purity nano magnesium aluminum silicate, 0.5 parts of graphite powder and 0.7 parts of polymer water-absorbing resin; wherein the polymer water-absorbing resin is provided by Guangzhou Yecheng Chemical Co., Ltd., has a particle size of 40-60 μm, and its water absorption multiple is 150 times.

[0049] Example 1

[0050] A continuous extrusion-molded ultra-high performance cement-based tile, the raw materials of which include cement, silica fume, mineral powder, fly ash microbeads, ceramic sand, modified machine-made sand, steel fiber, nano-modified component, water reducing agent, shrinkage compensating component, and cellulose ether; the specific preparation process is as follows:

[0051] 1) Weigh each raw material in proportion; each raw material and its weight proportion are: 700 parts of cement, 160 parts of silica fume, 120 parts of mineral powder, 80 parts of fly ash microspheres, 1000 parts of modified machine-made sand, 150 parts of steel fiber, 6 parts of composite modified component, 4 parts of water reducing agent, 22 parts of shrinkage compensating component, 2 parts of cellulose ether, and 185 parts of water;

[0052] 2) Stirring: Pre-disperse the modified components in 40% of the weighed amount of water to obtain mixture A. Weigh the other required raw materials and pour them into a mixer for dry mixing for 5 minutes. Add the remaining water and mixture A and stir for 18 minutes to obtain the blank required for tile making.

[0053] 3) Extrusion: The blank is poured into an extrusion cone hopper (1), and the lower part of the hopper is the inlet of an ultra-high performance cement-based tile extruder. The blank is extruded through a vacuum screw extruder (2) and transported to a corrugated extrusion port (3). The blank is then extruded through a transition conveying device (4) and sent into a tile mold (5). The extruder adopts a vacuum twin-screw extrusion process, with an extrusion pressure of 4.0 MPa and a vacuum degree of 10 - 3 Pa, extrusion rate 700mm / min.

[0054] 4) Cutting: The tile mold running speed is consistent with the extrusion speed. When the infrared sensing device (7) senses the front end of the tile film, the synchronous cutting machine (6) is started to cut the tile blank. The cutting machine is consistent with the tile mold speed along the conveyor belt direction (along the tile mold length direction), and cuts at a uniform speed perpendicular to the conveyor belt direction (along the tile mold width direction). After cutting, the cutting machine moves in the opposite direction along the conveyor belt and resets to the opposite side of the original position; reciprocating cutting is performed in this way.

[0055] 5) Curing: Transfer the tile mold and the tile blank to the bracket and send them to the steam curing room for 60℃ steam curing for 48 hours.

[0056] 6) Demolding: After curing, use a suction cup to remove the tile from the tile mold and color it to obtain the finished ultra-high performance cement-based tile (see the actual picture) Figure 2 ; It has a corrugated structure, thickness 6mm and width 998mm).

[0057] Example 2

[0058] A continuously extruded ultra-high performance cement-based tile, the preparation method of which is substantially the same as that of Example 1, except that the raw materials and their weight proportions are: 750 parts of cement, 200 parts of silica fume, 110 parts of mineral powder, 90 parts of fly ash microbeads, 1000 parts of modified machine-made sand, 140 parts of steel fiber, 7 parts of composite modified component, 5 parts of water reducer, 24 parts of shrinkage compensating component, 3 parts of cellulose ether, and 200 parts of water.

[0059] Example 3

[0060] A continuously extruded ultra-high performance cement-based tile, the preparation method of which is substantially the same as that of Example 1, except that the raw materials and their weight proportions are: 800 parts of cement, 160 parts of silica fume, 100 parts of mineral powder, 100 parts of fly ash microbeads, 1000 parts of modified machine-made sand, 130 parts of steel fiber, 8 parts of composite modified component, 5 parts of water reducer, 26 parts of shrinkage compensating component, 5 parts of cellulose ether, and 208 parts of water.

[0061] Comparative Example 1

[0062] A cement-based tile, whose preparation method is roughly the same as that of Example 1, except that the raw materials and their weight proportions are: each raw material is replaced by ordinary raw materials such as cement, sand, and water, and the weight proportions are: 100 parts of PO42.5 cement, 120 parts of river sand, and 35 parts of water.

[0063] Comparative Example 2

[0064] A cement-based tile, whose preparation method is roughly the same as that of Example 1, except that the raw materials and their weight proportions are: 700 parts of cement, 160 parts of silica fume, 120 parts of mineral powder, 80 parts of fly ash microbeads, 1000 parts of modified machine-made sand, 150 parts of steel fiber, 4 parts of water reducer, 22 parts of shrinkage compensating component, 2 parts of cellulose ether, and 185 parts of water.

[0065] Comparative Example 3

[0066] A cement-based tile, whose preparation method is roughly the same as that of Example 1, except that the raw materials and their weight proportions are: 700 parts of cement, 160 parts of silica fume, 120 parts of mineral powder, 80 parts of fly ash microbeads, 1000 parts of machine-made sand, 150 parts of steel fiber, 6 parts of composite modified components, 4 parts of water reducer, 22 parts of shrinkage compensating components, 2 parts of cellulose ether, and 185 parts of water; the machine-made sand used is ordinary 20-70 mesh machine-made sand.

[0067] Comparative Example 4

[0068] A cement-based tile, whose preparation method is roughly the same as that of Example 1, except that the raw materials and their weight proportions are: 700 parts of cement, 160 parts of silica fume, 120 parts of mineral powder, 80 parts of fly ash microbeads, 1000 parts of modified machine-made sand, 150 parts of steel fiber, 6 parts of composite modified components, 4 parts of water reducer, 22 parts of shrinkage compensating components, 2 parts of cellulose ether, and 185 parts of water; wherein the composite modified component is obtained by compounding graphite powder and high molecular water-absorbing resin in a mass ratio of 0.5:0.7.

[0069] Comparative Example 5

[0070] A cement-based tile, the preparation method of which is substantially the same as that of Example 1, except that the raw materials and their weight proportions are: 700 parts of cement, 160 parts of silica fume, 120 parts of mineral powder, 80 parts of fly ash microbeads, 1000 parts of modified machine-made sand, 150 parts of steel fiber, 6 parts of composite modified components, 4 parts of water reducer, 22 parts of shrinkage compensating components, 2 parts of cellulose ether, and 185 parts of water; wherein the composite modified component is obtained by compounding nano magnesium aluminum silicate and a polymer water-absorbing resin in a mass ratio of 1:0.7.

[0071] Comparative Example 6

[0072] A cement-based tile, whose preparation method is substantially the same as that of Example 1, except that the raw materials and their weight proportions are: 700 parts of cement, 160 parts of silica fume, 120 parts of mineral powder, 80 parts of fly ash microbeads, 1000 parts of modified machine-made sand, 150 parts of steel fiber, 6 parts of composite modified components, 4 parts of water reducer, 22 parts of shrinkage compensating components, 2 parts of cellulose ether, and 185 parts of water; wherein the composite modified component is obtained by compounding nano-magnesium aluminum silicate and graphite powder in a mass ratio of 1:0.5.

[0073] In order to verify the production feasibility and mechanical performance indicators of a continuously extruded ultra-high performance cement-based tile obtained in Examples 1 to 3, relevant performance tests were carried out on Examples 1 to 3 and Comparative Examples 1 to 6 with reference to GB / T 7019-2014 "Test methods for fiber cement products" and J / CT 567-2008 "Glass fiber reinforced cement corrugated tiles and ridge tiles". The results are shown in Table 1.

[0074] Table 1 Performance test results of Examples 1 to 3 and Comparative Examples 1 to 6

[0075]

[0076]

[0077] Through the embodiments and comparative examples, it can be found that by adopting the technical means of the present invention, a continuously extruded ultra-high performance cement-based tile can be realized, the lateral flexural strength reaches more than 5000N / m, the longitudinal flexural strength reaches more than 800N, and the maximum length reaches 5 meters. Compared with the traditional extrusion method that can only produce small pieces of cement tiles, the tiles produced by the present invention have been significantly improved in quality and size, and can be applied to the roofing system of large-span industrial plants.

[0078] The present invention is not limited to the above-mentioned embodiments. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention. The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.

Claims

1. A continuously extruded ultra-high performance cement-based tile, characterized in that: The required raw materials and their weight proportions include: 650-800 parts of cement, 160-200 parts of silica fume, 100-130 parts of mineral powder, 60-100 parts of fly ash microbeads, 1000 parts of modified machine-made sand, 120-150 parts of steel fiber, 4-9 parts of composite modified components, 3-6 parts of water reducer, 20-30 parts of shrinkage compensating components, 2-6 parts of cellulose ether, and 180-230 parts of water; the composite modified components include nano magnesium aluminum silicate, graphite powder and polymer water-absorbing resin; the modified machine-made sand is machine-made sand after ball milling, screening and hydrophobic modification; The mass ratio of the nano magnesium aluminum silicate, graphite powder and polymer water-absorbing resin is 1:0.3-0.7:0.3-0.

8.

2. The ultra-high performance cement-based tile according to claim 1, characterized in that: The screening step is to screen out granules with a particle size of 20-70 mesh; the ball milling step adopts a ball milling rate of 50-70 r / min and a time of 40-80 s.

3. The ultra-high performance cement-based tile according to claim 1, characterized in that: In the hydrophobic modification step, the machine-made sand is soaked in a silane coupling agent solution; the silane coupling agent is isooctyltriethoxysilane coupling agent or methyltrimethoxysilane.

4. The ultra-high performance cement-based tile according to claim 1, characterized in that: The shrinkage compensating component is mainly composed of sulphoaluminate clinker and magnesium oxide, which are compounded in a mass ratio of 8-12:4-5.

5. The ultra-high performance cement-based tile according to claim 1, characterized in that: The cement is silicate cement; the silica fume SiO2 content is ≥96%, and the 28d activity index is ≥110%; the 28d activity index of the mineral powder is ≥105%; the water demand ratio of the fly ash microspheres is ≤95%, the 28d activity index is ≥96%, and the glass content is ≥90%.

6. The ultra-high performance cement-based tile according to claim 1, characterized in that: The steel fiber has a length of 5-6 mm and a diameter of 0.1-0.12 mm.

7. The ultra-high performance cement-based tile according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid high-efficiency water reducing agent, and its water reducing rate is 25-30%.

8. The preparation process of the ultra-high performance cement-based tile according to any one of claims 1 to 7, characterized in that: The steps include: 1) Mixing: Add the modified component to part of the water to obtain a mixture A, dry-mix the other raw materials except water, add the remaining amount of water and the mixture A, and stir to obtain a blank; 2) Extrusion: Use a vacuum screw extruder to extrude the obtained blank into a tile mold and cut it; 3) Curing: The obtained green tile with the tile mold is subjected to steam curing and demolding to obtain the ultra-high performance cement-based tile.

9. The preparation process according to claim 8, characterized in that: The steam curing temperature is 60-90° C. and the time is 36-60 hours.